Jonghwan Moon
Product group
Detection & Utilities

Leak detection fluid is easily taken for a mild liquid that only makes bubbles and left in place after the test, but what it contains concentrates where it dries and can corrode or crack the metal. What actually lies behind the damage can be chloride and sulphur, ammonia that cracks brass, residue built up in gaps, skipped cleaning or hot piping, and sometimes two or more at once.

Background

Only a few weeks after a pressure test, the brass fittings that were sprayed with leak detection fluid show blue-green powder and white residue around the nuts, with fine cracks. On stainless steel piping, pinhole corrosion can follow the line where the fluid ran down and gathered. The fluid used to find leaks has made new ones, so parts must be replaced and the system retested at a cost in time and money, and on gas or refrigerant lines a crack that leaks is a safety problem. In a case examined by the U.S. National Bureau of Standards, flexible brass gas appliance connectors failed within three to six weeks of installation, with cracks through the wall at both ends, where leak detector would presumably have been applied (Ambrose & Kruger, 1975).

Leak detection fluid is usually water with surfactants dissolved in it, and its job is to make bubbles where gas escapes. The trouble starts once the water dries. The other ingredients stay behind and concentrate, and repeated application and drying at the same spot concentrates them further (ASTM International, 2021). Stress corrosion cracking is cracking of a metal under tensile stress in contact with a particular substance, even where little corrosion shows on the surface. In austenitic stainless steels, how readily it occurs depends strongly on temperature, chloride concentration and pH (Vakili et al., 2024). So the same fluid may do nothing at all on one part and crack another before long, depending on material, stress and temperature.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: check the fluid's safety data sheet, the SDS, and technical data sheet, the TDS, for its ingredients, pH, and the materials and temperature range it suits, then log the material of the corroded part, when and how often fluid was applied there, and whether it was cleaned after the test, and compare the two.

Hypothesis 1: chloride and sulphur

Look at this hypothesis when a general-purpose fluid was used on stainless steel, nickel alloy or high-chromium alloy parts without checking what is in it, or when soapy water was mixed on site from detergent. It applies especially where tensile stress remains, at welds, bent tube and tightly made-up compression fittings, and on the underside where fluid runs down and gathers. Picture a new run of stainless instrument tubing, with whatever leak detector was to hand sprayed on every fitting and the job signed off once no bubbles showed. At the next routine inspection, a brown rust streak runs down from each fitting along the path the fluid took, ending in a pinhole.

Stainless steel resists rust thanks to a very thin oxide film on its surface. Chloride ions break this film down in places, producing narrow, deep pits, and where tensile stress acts there, the pits can lead on to stress corrosion cracking (Vakili et al., 2024). Sulphur does harm by another route. In nickel and nickel alloys, sulphur gathering at the boundaries between grains has been reported as a cause of embrittlement at high temperature (Bricknell et al., 1982). That is why the bubble leak testing standard requires the test fluid for parts containing stainless steel, nickel or chromium alloys to hold sulphur and halogens, elements such as chlorine and fluorine, below 10 ppm each, and one public laboratory's test procedure uses the same limit (ASTM International, 2022; LANL, 2018).

Start with the paperwork for the fluid. See whether the SDS and TDS state that it may be used on stainless steel or nickel alloys and give its sulphur and halogen content, and if not, ask the supplier for a certificate of analysis. Soapy water made on site has unknown contents, so treat it as suspect. Then look at the damage. Check whether the pits and stains line up with the fittings that were sprayed and the places where fluid ran and gathered, and scrape the surface deposit into a sample for laboratory analysis of chloride and sulphur. If cracking is suspected, confirm it with penetrant testing or a cross-section.

When the ingredients look responsible, change the fluid first. Write into the procedure that stainless steel and nickel alloy systems take only fluid labelled low in sulphur and halogens and backed by a certificate, and stop using detergent-based soapy water. Check the depth of existing pits to decide which parts to replace, and inspect every other place the same fluid was used. Even with the new fluid, keep rinsing it off once the test is over.

Hypothesis 2: ammonia on brass

Suspect ammonia when cracks appear in brass fittings, valves or flare nuts on gas, refrigerant or compressed air lines. Typical cases are nuts tightened hard or undone and retightened several times, brass tube bent during installation, and a strongly smelling alkaline fluid or a detergent of unknown origin. Say a factory compressed air line is being extended, with brass ball valves and nipples made up tight and the joints checked with leak detector found in the store. Not long after, several nipples on the same run split along the thread roots and start to hiss.

Brass is an alloy of copper and zinc, and ammonia reacts with copper to form copper-ammonia compounds. Most brasses can suffer stress corrosion cracking from as little as trace ammonia in the air when four things are present together: ammonia or one of its derivatives, moisture, oxygen and stress. In the connector case above, the leak detector smelled strongly of ammonia and had a pH of 10.0, the residue contained a compound expected when copper reacts with ammonia, and the tubing carried residual stress from fabrication or installation (Ambrose & Kruger, 1975). The stress side has its own conditions. Soft brass is not considered susceptible to ammonia stress corrosion, but work-hardened brass is, over-tightening a nut can put a part into that state, and the problem grows in older parts tightened many times (ASTM International, 2021). The conditions under which brass cracks in ammonia solutions have long been analysed in terms of the solution's potential and pH (Mattsson, 1961).

Checks run on both the fluid and the part. Look in the SDS ingredient list for ammonia, ammonium salts and amines, note whether the bottle smells of ammonia when opened, and test with pH paper for strong alkalinity. On the part, look for blue-green corrosion product around the crack and whether the crack sits where stress concentrates, at a thread root or a bend. Whether parts from the same lot carry enough residual stress to crack can be checked with a standard test that exposes them to ammonia vapour. The test relies on a condensed film rich in copper complex ions forming on the surface and driving the cracks (ASTM International, 2018).

Once ammonia is confirmed, withdraw that fluid from copper alloy systems and switch to one stated to have been evaluated with the standard test for brass stress corrosion. List and inspect every brass part the old fluid touched, even where no crack shows, and replace the cracked ones. Make up fittings to the set tightening standard rather than beyond it, and put parts that have been undone and retightened many times at the top of the replacement list.

Hypothesis 3: built-up residue

Check for built-up residue on equipment where the same fittings are retested at every inspection, in narrow gaps that rinse water hardly reaches, such as threads, flares, lapped plates and the edges of weld beads, and wherever a fluid that leaves a lot of solids after drying is used. Take a plant where, at every shutdown, the threaded end of the same pressure-reducing valve body has been sprayed and only the outside wiped with a dry cloth. Each thread root holds layer on layer of whitish film, and the metal beneath it, once the film is lifted, has turned dark.

Fluid that gets into a narrow gap is out of reach of a wipe, and when it dries it leaves its ingredients there. The standard test for brass applies fluid to a specimen and lets it dry again and again, which concentrates the ingredients and quickly reproduces a system being tested many times over its life (ASTM International, 2021). The specification for oxygen-system leak detection compound limits the residue left after drying to 0.50% and tests separately whether a panel with dried fluid rinses clean in cold deionised water, and whether fluid placed in the gap between two clamped panels corrodes them more than untreated panels (DoD, 1998). The concentration can be large. At wet and dry interfaces, chloride at a few ppm in solution can build up to hundreds of ppm where it evaporates (SSINA, n.d.).

First see whether the corrosion is concentrated in gaps, thread roots and low spots where fluid collects. Spraying a little water on the white film shows whether it foams, which suggests dried surfactant. In the connector case too, the white residue foamed when sprayed with water and tested alkaline, and was judged probably to be some kind of detergent (Ambrose & Kruger, 1975). Count from the inspection records how many times that spot has been tested, and check whether the fluid's data give a residue content.

The remedy starts with lifting that film: rinse the spot thoroughly with water, then dry it. On parts with many gaps, cut the amount down to a thin coat brushed on, and revise the checklist so that every retest at a repeat spot includes rinsing and drying as one step. Consider at the same time a fluid that leaves few solids and rinses off easily.

Hypothesis 4: skipped cleaning

Where the procedure has no cleaning step after the test, where parts are only blown dry, or where fluid is left on and covered with insulation, tape or paint, look first at skipped cleaning. Rinsing with tap water or groundwater and leaving it there belongs here too. On a day when commissioning was running late, the insulators came in the moment the pressure test ended and lagged the fittings. The fluid was shut inside the insulation with no chance to wipe it off, and at the next shutdown, with the lagging stripped, rust stains show only on the sections that had been covered.

Once the test is over, the fluid has done its job and there is no reason to leave it. One public laboratory's bubble test procedure requires the solution to be removed after testing, using materials and methods suited to the item (LANL, 2018). Fluid left in place dries to its ingredients alone, and when moisture reaches it again it becomes a concentrated solution wetting the metal. Insulated sections are worse. Wet insulation can carry corrosive ions and collect them on a hot stainless steel surface, and heat drives off water and speeds up reactions (ASTM International, 2023). The rinse water deserves thought as well; the corrosion test in the oxygen-system specification rinses with cold deionised water (DoD, 1998).

Skipped cleaning shows up when the records are set against where the corrosion sits. See whether the procedure and work records include rinsing and drying after the test, and whether anyone signed to say it was done. Then compare whether corrosion appears only where something was put over the fittings after the test, under insulation, tape or paint, while the same kind of fitting left uncovered is sound. Check the chloride level of the rinse water too.

Where cleaning was skipped, add a step to the procedure for rinsing with clean water and drying after the test, with a box to sign. Rinse stainless steel systems with low-chloride water, and change the work sequence so that insulation or painting starts only after the surface has been confirmed dry. Open up sections already covered as far as practicable, and where rust shows, review the cause again alongside the other hypotheses.

Hypothesis 5: hot piping

Temperature may have played a part when steam lines, hot water lines or heat exchangers are checked hot while running, or when piping goes up to operating temperature soon after the test. The scene is a steam header being brought back up to heat after a shutdown, with fluid sprayed on every flange and fitting to find leaks. The fluid steams off and dries almost as soon as it lands, leaving only white rings on the surface.

On a hot surface water leaves fast, so the fluid's ingredients concentrate straight away where it was applied. Chloride stress corrosion cracking of stainless steel is rare below 60 °C under immersion, but where chloride-bearing liquid evaporates on a hot surface it can occur at temperatures well below that (SSINA, n.d.). One review concludes that such cracking can start at about 20 °C and that crack growth speeds up sharply above 60 °C (Vakili et al., 2024). The bubble test has its own temperature conditions as well. One public laboratory's procedure keeps the surface between 40 °F and 125 °F, about 5 °C to 50 °C, throughout the examination, and requires the solution to suit the test temperature (LANL, 2018).

Find the surface temperature at the time of testing in the records, or measure it with a contact thermometer at the next test. Compare whether corrosion and white marks cluster on hot sections, especially those checked while running, while cool sections done with the same fluid are sound. Check the working temperature range in the fluid's TDS as well.

The rule is to test only once the surface is back within the procedure's temperature range. For systems that must be checked hot, use a fluid made for that temperature or consider a leak test method that applies no liquid. Either way, rinse the fluid off and dry the surface before bringing the system up to operating temperature.

Finding the cause

Five hypotheses do not mean five separate investigations. Start with what the paperwork can settle. Setting the fluid's SDS and TDS against the part material shows at a desk whether a fluid without a sulphur and halogen statement went on stainless steel or nickel alloy, or a fluid containing ammonia went on brass. If the work records show whether cleaning was done and what the surface temperature was, those can be ruled out before anyone goes to the plant.

Next come the form and location of the damage. Cracks at thread roots or bends in brass fittings, with blue-green product around them, point first to ammonia. Pitting on stainless steel along the path where fluid ran and gathered points to chloride, and corrosion confined to gaps and thread roots to built-up residue. Rust found only where something was put over the part after the test points to skipped cleaning, and damage clustered on hot sections with white marks to heat.

If that still does not settle it, run a comparison. Applying the old fluid and a different one to specimens of the same material, with repeated drying, separates a problem with the fluid itself from a problem with how it is used. For brass there is a standard test that evaluates fluids in just this way, so the work can go to a test laboratory (ASTM International, 2021). Laboratory analysis of the corrosion product for chloride, sulphur and copper-ammonia compounds narrows down which ingredient was at work.

The final check is that the damage does not come back at the same spot. After changing the fluid or the procedure, look again at the same fittings and gaps over the first few inspections; the cause is fixed only when no new stains or cracks appear. Keeping the change and the inspection results in one record makes comparison easier if a similar symptom turns up later.

The hypotheses can overlap. On hot piping where a chloride-bearing fluid was used, left unrinsed and covered with insulation, ingredients, cleaning and temperature all meet in one place. Changing the fluid is then not enough; rinsing and drying must go into the procedure and the test temperature must be respected as well. If the damage returns after only one of these is fixed, another cause is still there.

Limits and cautions

Ingredient limits and working temperature ranges for leak detection fluids differ by product and by the governing standard, so numbers follow the product's SDS and TDS and the standard that applies to the system. The standard test for brass applies only to brass, and passing it does not mean a fluid is acceptable for stainless steel or aluminium alloys (ASTM International, 2021). Deciding why a part cracked is work for a metallurgical laboratory, and if cracks appear on gas or pressurised piping, do not keep it in service on floor judgement; take it out of use and have a qualified person confirm its condition.

Safety matters too. Follow the SDS for protective equipment when handling leak detection fluids and rinsing chemicals, and handle fluids that smell strongly of ammonia where there is ventilation. Keep time spent close to pressurised parts short, and undo or replace cracked parts only after the system is fully depressurised and isolated.

Sources

  1. Ambrose, J. R., & Kruger, J. (1975). Failure of flexible brass gas appliance connectors (NBSIR 75-669). National Bureau of Standards. https://nvlpubs.nist.gov/nistpubs/Legacy/IR/nbsir75-669.pdf
  2. ASTM International. (2018). ASTM B858-06(2018), Standard test method for ammonia vapor test for determining susceptibility to stress corrosion cracking in copper alloys. https://store.astm.org/b0858-06r18.html
  3. ASTM International. (2021). ASTM G186-05(2021), Standard test method for determining whether gas-leak-detector fluid solutions can cause stress corrosion cracking of brass alloys. https://store.astm.org/g0186-05r21.html
  4. ASTM International. (2022). ASTM E515-11(2022), Standard practice for leaks using bubble emission techniques. https://store.astm.org/e0515-11r22.html
  5. ASTM International. (2023). ASTM C692-13(2023), Standard test method for evaluating the influence of thermal insulations on external stress corrosion cracking tendency of austenitic stainless steel. https://store.astm.org/c0692-13r23.html
  6. Bricknell, R. H., Mulford, R. A., & Woodford, D. A. (1982). The role of sulfur in the air embrittlement of nickel and its alloys. Metallurgical Transactions A, 13(7), 1223–1232. https://doi.org/10.1007/BF02645505
  7. Los Alamos National Laboratory [LANL]. (2018). ITM-1306-NDE-LT-101, Bubble leak testing: Direct pressure & vacuum box (Rev. 0). LANL Engineering Standards Manual STD-342-100. https://engstandards.lanl.gov/esm/welding/vol6/ITM-1306-NDE-LT-101-R0.pdf
  8. Mattsson, E. (1961). Stress corrosion in brass considered against the background of potential/pH diagrams. Electrochimica Acta, 3(4), 279–291. https://doi.org/10.1016/0013-4686(61)85004-4
  9. Specialty Steel Industry of North America [SSINA]. (n.d.). Chloride stress corrosion cracking. Retrieved November 2026. https://www.ssina.com/education/corrosion/chloride-stress-corrosion-cracking/
  10. U.S. Department of Defense [DoD]. (1998). MIL-PRF-25567E, Performance specification: Leak detection compound, oxygen systems. https://everyspec.com/MIL-PRF/MIL-PRF-010000-29999/MIL-PRF-25567E_2163/
  11. Vakili, M., Koutník, P., Kohout, J., & Gholami, Z. (2024). Analysis, assessment, and mitigation of stress corrosion cracking in austenitic stainless steels in the oil and gas sector: A review. Surfaces, 7(3), 589–642. https://doi.org/10.3390/surfaces7030040

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.