KALTECKOREA

BlogApplication notes

Why does low-residue maintenance fluid strip paint and markings?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Maintenance Aids

Blaming whoever rubbed too hard, or just switching to another cleaner, is the usual response when paint or markings come off, but removal is set by the solvent, the coating, the ink, the way it is wiped and the surface temperature together, so changing one tends to let it happen again elsewhere. What actually lies behind it can be a strong solvent that dissolves or swells the coating, under-cured paint, rubbing force and time, inks and labels that cannot take solvent, or a hot surface, and sometimes two or more at once.

Background

During an equipment inspection, oil smears are wiped off with low-residue maintenance fluid, but paint colour comes away on the rag and the wiped area has lost its gloss. The lettering on the nameplate beside it has smeared, and the rotation arrow and warning marks have faded. Where the coating has thinned or come off, rust can start and touch-up painting becomes necessary, and once rating plates, safety signs and pipe identification marks can no longer be read, that leaves an immediate gap in inspection and safety management.

Low-residue maintenance fluid is made of volatile solvents that evaporate completely so nothing is left after wiping (Durkee, 2014). The very property that makes it good at dissolving oil also acts on the polymers that paints and inks are built on. How much a solvent swells or dissolves a polymer can be judged by how alike the two are in the nature of their intermolecular forces, and Hansen solubility parameters express this in numbers (Hansen, 2007). A polymer does not dissolve the moment solvent touches it; it goes through stages in which the solvent soaks in, the polymer swells and its chains work loose (Miller-Chou & Koenig, 2003).

So what comes off is not decided by one thing. It depends together on how well the coating and ink resist that solvent, how long and on how warm a surface the solvent stays, and how much rubbing happens in that time.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: check the solvent content and material compatibility guidance in the fluid's safety data sheet, the SDS, and technical data sheet, the TDS, and set them beside a record of the paint type and painting date of the damaged surface, the printing method and label specification of the markings, and how the wiping was done and what state the surface was in.

Hypothesis 1: solvent too strong

This hypothesis comes first right after a change to a different maintenance fluid, when using a product that contains ketones or aromatic solvents, and when the surface is a paint that can redissolve even after drying, such as a lacquer or acrylic, or a touch-up spray paint applied on site. In the first week after supply problems forced a switch to another low-residue fluid, an operator wipes oil marks off a grey machine cover as always. The wiping is no different, but this time the rag turns grey.

Paints split in how they respond to solvent according to how they harden. A thermoplastic film, which hardens only as the solvent leaves and the polymer chains tangle, redissolves when it meets a suitable solvent, while a crosslinked film, whose chains are joined into a network by chemical reaction, does not dissolve but can take up solvent and swell (Jones et al., 2017). How strongly each solvent acts varies widely. In a study that immersed oil paint films in many solvents, aliphatic hydrocarbons caused little swelling, toluene and xylene were stronger, and acetone was among the fastest-acting. The same study explains that in a swollen film the binder holds the pigment less firmly, so pigment is easily lifted off by a cleaning swab (Phenix, 2002). The solvent power of hydrocarbon solvents is compared by a standard test value called the kauri-butanol value, and a higher value means a stronger solvent (ASTM International, 2021a).

Check in an inconspicuous spot. Hold a white cloth wetted with the same maintenance fluid against the painted surface, rub back and forth a set number of times, then see whether colour has come off on the cloth and whether the film has softened or lost gloss. Rubbing with a wetted cloth like this to judge a coating's solvent resistance is set out as a standard practice (ASTM International, 2019). Rub the spot right next to it the same way with the product used before the switch, compare the two results side by side, and see in the two SDSs how the solvent content has changed.

If colour comes off only with the new fluid, stop using it on painted surfaces. Where painted surfaces are wiped often, use the same rub test to pick a fluid that attacks the coating less, and ask the fluid supplier for compatibility data on that paint. Keeping separate fluids for painted surfaces and for metal parts makes a repeat unlikely.

Hypothesis 2: under-cured paint

Coatings are easily left under-cured on surfaces painted new or touched up during maintenance only a short time ago, when the mixing ratio of a two-part paint has drifted, when painting was done on a cold or damp day, and when a thick coat went on in one pass. A pump base repainted during a scheduled shutdown is one example. At the trial run a few days later oil splashes onto it, and when it is wiped with low-residue fluid the film smears stickily and bare metal shows along the rag marks.

Paints that change chemically as they cure, such as epoxies, urethanes and alkyds, build solvent resistance as curing proceeds, and the time to reach a given level depends on temperature, film thickness, air movement and, for water-borne or moisture-curing paints, humidity (ASTM International, 2019). A film whose chains are not yet fully crosslinked has a looser network, so solvent gets in more easily and the film swells more (Jones et al., 2017). So a fluid the fully cured film would have withstood softens the under-cured film until the rag pushes it off.

First compare the painting date and the temperatures since then with the full-cure time and conditions in the paint TDS. For a two-part paint, find the mixing ratio and how long the mix was used after mixing in the records. Press a fingernail into the film to see whether it leaves a mark, and run a rub test with the solvent and number of rubs set by the paint maker; but since some paints gain solvent resistance before they are cured enough for service, do not conclude from a passed rub test that the paint is fully cured (ASTM International, 2019).

If the film looks under-cured, do not wipe that surface with solvent until the full-cure time has passed; use a dry cloth or a cleaner that does not attack the paint. A film that never cures has to be repainted after correcting the cause, such as the mixing ratio or the painting temperature. After touch-up painting, write into the work standard when the surface may first be wiped with solvent.

Hypothesis 3: hard, long rubbing

With the same fluid, the amount removed changes greatly when a coarse pad is used to shift hardened oil or baked-on grime, when a soaked rag is left on the surface to soften the dirt, and when the same spot is wiped over and over. Think of cleaning time at the end of a shift. An operator lays a rag soaked with fluid on a control cabinet door, does another job, then comes back and rubs hard for a long time. Only the rubbed area has lost its gloss, with the colour underneath showing through.

Solvent and force feed each other. The longer solvent stays, the deeper it soaks in and the more the film swells and softens, and polymers dissolve away through these stages over time (Miller-Chou & Koenig, 2003). In a swollen film the resin holds the pigment less firmly, so rubbing with the same force lifts pigment more easily (Phenix, 2002). The standard practice for judging a coating's solvent resistance also fixes how many double rubs are made with the wetted cloth and states the result as that count, because the number and manner of rubs change the outcome (ASTM International, 2019).

Look at the shape of the damage. If streaks follow the direction the rag travelled, or the gloss has gone in the outline of where the rag was left lying, suspect force and time first. Wipe the spot right beside it just once, lightly, with a soft cloth wetted with the same fluid; if no colour comes off then, the way of wiping is closer to the cause than the fluid itself.

Here the thing to change is the method rather than the fluid. Put the fluid on the rag, do not leave soaked rags lying on painted surfaces, wipe briefly with a soft cloth, and follow with a dry cloth before it dries. Scrape hardened grime off first with a plastic scraper or soften it with a cleaner that does not attack the coating, use the fluid only for the final wipe, and keep coarse pads off painted surfaces.

Hypothesis 4: fragile inks and labels

If the paint is fine but the lettering has gone, look at the printing and labels: rating plates on motors and pumps, inspection labels, pipe identification marks, gauge scales, inkjet-printed dates and numbers, and screen-printed control markings. A single pass with a fluid-wetted cloth over an inspection label beside the rotation arrow on a pump cover, and the ink has smeared so the date cannot be read, while the edges of the label lift and curl up.

How well printed matter resists solvent depends on the ink, the printing method and the substrate, and there is an international standard for assessing how far prints, from offset, screen, gravure and flexo to inkjet, resist agents including solvents (ISO, 2021). In a label, ink, film and adhesive all have to hold up, and the standard for markings and labels fixed to equipment checks that lettering is still legible after chemical exposure and that the label does not curl or lift at the edges (ULSE, 2025). Ink resins and adhesives are polymers too, so they swell or dissolve on meeting a solvent with similar solubility properties, on the same principle as coatings (Hansen, 2007).

Check in the label specification or supplier data which chemical exposure tests the label has passed. If spare labels or samples printed the same way are available, rub them with a cloth wetted with the same fluid and see whether the ink smears, the film clouds over or the adhesive oozes at the edges. Standards for evaluating how plastics resist chemicals also fix the immersion time and temperature as test conditions, so match the check to the wiping time and temperature on the floor (ASTM International, 2021b).

Start by steering clear of fragile labels and markings. Put only a little fluid on the cloth and wipe around them. Where maintenance fluid reaches often, use labels that have passed solvent exposure tests or labels under a clear protective film, and for markings that must stay legible for years, such as rating plates, consider engraving or metal plates. Replace or remake faded safety signs and nameplate information straight away.

Hypothesis 5: hot surface

Wiping surfaces that have not yet cooled, such as motor and pump casings just after shutdown, moulds and the covers round them, steam or hot-water pipes and oven doors, can give a different result from wiping them cold. A typical case is wiping oil off a mould cover right after production stops, while it is too warm to keep a hand on for long. The same fluid on the same spot did nothing when cold, but now the film turns tacky and colour comes off on the rag.

A coating changes sharply as it passes its glass transition temperature, where the cured resin goes from a hard, glassy state to a soft, rubbery one. Closer to this temperature, the polymer chains move more freely, the film softens and solvent soaks in faster (Jones et al., 2017). So with the same fluid and the same rubbing, coatings and inks on a hot surface can swell and smear off sooner. The heat resistance in a paint TDS is the temperature the film withstands under heat alone, so do not read it as meaning the film also withstands solvent at that temperature. Even if the solvent flashes off quickly from the hot surface, a fluid-wetted rag keeps feeding solvent to the spot, so the effect does not go away.

Measure and record the surface temperature at the time of wiping with an infrared thermometer, and compare it with the heat resistance or glass transition data in the paint TDS. See in the records whether the damage clusters in wiping done right after running, and wipe the same spot once it has cooled, with the same fluid and the same method; comparing the results shows how much temperature contributes.

The simplest remedy is to move the wiping to after the surface has cooled. Decide the temperature below which wiping is allowed from the paint and fluid TDSs, and on hot surfaces that must be wiped during operation use only cleaners stated as suitable for hot surfaces. Right after running, take off the oil with a dry cloth only, and leave solvent wiping to the next maintenance, when the surface is cold.

Finding the cause

The five hypotheses do not each need a separate test. Whether the fluid was changed, when the surface was painted and whether it was hot when wiped can be confirmed quickly from records and memory, and the rub test can then be done in an inconspicuous spot. Sample tests and label replacement come last.

What came off is the first clue. If the paint is fine and only lettering or labels are damaged, look first at the inks and labels; if the film smears only on freshly painted surfaces, look first at under-curing. If colour comes off here and there even on old paintwork, suspect the fluid's solvent power, and if the damage follows the rag's strokes or the outline of a rag left lying, suspect rubbing force and time. Damage only where wiping followed straight after running points to surface temperature.

Timing comes next. If the damage began when the fluid was changed, the fluid is the likelier cause; if it happens only within days of touch-up painting, curing is. If results differ from person to person, the wiping methods differ, so compare how each operator wipes. Conversely, if the same person wiped the same spot with the same fluid and the damage appeared only on certain days, check whether the equipment had just stopped on those days and whether the surface had been repainted in between.

If that still does not settle it, run control trials that change one thing at a time. On the same cold surface, rub the same number of times with the fluid used before and after the change; compare a spot wiped once lightly with the same fluid against one wiped hard and long; and wipe the same spot warm and cold. The final check is to see that paint and markings suffer no further damage after a period of wiping with the chosen fluid and method.

The hypotheses often overlap. Rubbing an under-cured film hard and long with a strong fluid while it is hot puts four causes to work at once, and fixing only one of them may not improve the result much. In such cases, correct the easy things first, the wiping method and the timing, then change the fluid if damage continues, and leave decisions on recoating and relabelling until last.

Limits and cautions

Cure times and heat resistance of paints, chemical resistance of labels and material compatibility of fluids differ by product, so take numbers from each product's TDS and supplier data. The rub test is only a floor check to aid judgement; for coatings tied to corrosion protection or certification, and for legally required markings, get confirmation from the paint supplier and the person responsible for the equipment. Where rating plates or safety signs can no longer be read, confirm that information separately before using the equipment until the markings are restored.

Many of the solvents used in low-residue maintenance fluids ignite easily and can be harmful when breathed in or in frequent skin contact (OSHA, n.d.). Solvents such as acetone have flash points below room temperature (NIOSH, n.d.), so do not use them near hot surfaces or flames, and collect wet rags in a lidded metal container. Follow the product SDS for ventilation, protective gloves and safety glasses, and stop and lock out moving equipment before wiping.

Sources

  1. ASTM International. (2019). ASTM D5402-19, Standard practice for assessing the solvent resistance of organic coatings using solvent rubs. https://store.astm.org/d5402-19.html
  2. ASTM International. (2021a). ASTM D1133-13(2021), Standard test method for kauri-butanol value of hydrocarbon solvents. https://webstore.ansi.org/standards/astm/astmd1133132021
  3. ASTM International. (2021b). ASTM D543-21, Standard practices for evaluating the resistance of plastics to chemical reagents. https://store.astm.org/d0543-21.html
  4. Durkee, J. B. (2014). Cleaning with solvents: Science and technology. William Andrew, Elsevier. https://shop.elsevier.com/books/cleaning-with-solvents-science-and-technology/durkee/978-1-4557-3131-2
  5. Hansen, C. M. (2007). Hansen solubility parameters: A user's handbook (2nd ed.). CRC Press. https://doi.org/10.1201/9781420006834
  6. International Organization for Standardization [ISO]. (2021). ISO 2836:2021, Graphic technology — Prints and printing inks — Assessment of resistance of prints to various agents. https://www.iso.org/standard/76452.html
  7. Jones, F. N., Nichols, M. E., & Pappas, S. P. (2017). Organic coatings: Science and technology (4th ed.). Wiley. https://www.wiley-vch.de/en/areas-interest/natural-sciences/organic-coatings-978-1-119-02689-1
  8. Miller-Chou, B. A., & Koenig, J. L. (2003). A review of polymer dissolution. Progress in Polymer Science, 28(8), 1223–1270. https://doi.org/10.1016/S0079-6700(03)00045-5
  9. National Institute for Occupational Safety and Health [NIOSH]. (n.d.). NIOSH pocket guide to chemical hazards: Acetone. Retrieved November 2026. https://www.cdc.gov/niosh/npg/npgd0004.html
  10. Occupational Safety and Health Administration [OSHA]. (n.d.). Solvents. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/solvents
  11. Phenix, A. (2002). The swelling of artists' paints in organic solvents. Part 2, Comparative swelling powers of selected organic solvents and solvent mixtures. Journal of the American Institute for Conservation, 41(1), 61–90. https://cool.culturalheritage.org/jaic/articles/jaic41-01-005.html
  12. UL Standards & Engagement [ULSE]. (2025). UL 969, Standard for marking and labeling systems (6th ed.). https://webstore.ansi.org/standards/ul/ul969ed2025

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.