KALTECKOREA

BlogApplication notes

Why does paint or print not stick to parts moulded with release agent?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Release & Process Aids

Switching paint or ink is the usual response when coatings or print peel from moulded parts, but if release agent left on the surface already occupies the places the coating needs, whatever is applied tends to peel again. What actually lies behind it can be silicone release agent carried onto the part, too much spray, an under-cured semi-permanent coat, poor cleaning or unsuitable moulding conditions, and often two or more at once.

Background

Tape pressed onto a housing fresh from the paint line comes away with the paint film still stuck to it. Other parts show small round craters where the paint has been pushed back, and pad-printed lettering scrapes off under a fingernail. Such parts must be stripped and repainted or scrapped, and since the defect only shows after painting and drying, the cost of moulding, painting and drying up to that point is lost with them. If they slip past inspection and peel after shipping, the result is returns and lost customer trust.

Paint or ink sticks only if the liquid first wets the surface evenly and then attracts, bonds with, or soaks into and entangles with the molecules at the surface. Most industrial plastics, however, have low surface free energy and few polar groups, which makes them hard to bond to begin with, and that is why separate surface treatments such as plasma or chemicals are used (Awaja et al., 2009). A release agent is made to do exactly the opposite. Composite moulding research reports that release agent residues left on the part surface lower adhesion, and one model for thermoset composites holds that release agent diffuses into the resin during cure, with the time available for that diffusion as the main factor setting how much is carried over (Blass et al., 2017). In painting, such residues can show up as delamination over large areas or as point-like wetting defects called craters (Fraunhofer IFAM, n.d.).

Finding the cause of a paint failure therefore comes down to telling what is left on the part surface and how much, and whether the plastic beneath is in a state to accept the coating. The type and amount of release agent, the state of the release film on the mould, cleaning, and the surface layer and stress formed in moulding all bear on this.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: set failed and good parts side by side, check the ingredients and directions for use of the release agent in its technical data sheet, the TDS, and its safety data sheet, the SDS, then compare the spray records, mould maintenance log, cleaning conditions and moulding settings for the failed lot against them.

Hypothesis 1: silicone transfer

On an injection line where release agent is sprayed onto the mould and parts go straight on to painting or printing, start with what the release agent contains. If the can or the SDS lists silicone, or polydimethylsiloxane, PDMS for short, this hypothesis moves to the front. The same holds for plants that handle silicone lubricants or silicone products under the same roof. Picture the day a new mould goes on: the first part will not come out cleanly, so the operator gives it one burst of the familiar silicone spray and carries on. The moulded parts look clean and feel no greasier than usual. The next day, on the paint line, only parts from this lot show round holes dotted across the paint film.

The trouble with silicone lies in what the molecule shows to the outside. A PDMS chain is sheathed in non-polar methyl groups, so it attracts polar liquids such as water and alcohols only weakly, and its surface energy is low. Even a crosslinked, cured silicone network keeps some unbound chains, and these can gather at the surface (Hauer et al., 2024). Silicone on the mould moves onto the part surface on contact with hot resin, and even spread too thin to see, it leaves places the paint cannot wet. Paint that meets such a place is pushed back into a crater, or if it covers it, has nothing to hold on to and lifts easily. In composite tests with PDMS films as thin as about 6 nm, measured surface contamination matched the failure pattern in the bond tests well (Palmieri et al., 2016).

First see how the part surface takes a liquid. Put a drop of water on several spots of good and failed parts, or draw a test pen filled with liquid of known surface tension across them, and see whether the line stays spread or pulls into beads. The method of measuring wetting tension with test liquids was standardised for polyethylene and polypropylene film, so on other plastics use it as a comparison against good parts (ASTM International, 2023a). Confirm any silicone content from the can and the SDS, and if the composition must be pinned down, send parts to a laboratory for X-ray photoelectron spectroscopy, or XPS, or time-of-flight secondary ion mass spectrometry, TOF-SIMS, which read the elements and molecules in the top few nanometres (Fraunhofer IFAM, n.d.).

If silicone looks to be the cause, review a switch to a silicone-free release agent with the supplier for any parts that will be painted or printed. Silicone left on the mould face, ejector pins and operators' gloves will keep transferring for a while after the switch, so clean the mould and check the first lot with a wetting test before it goes to paint. Assign a storage place for silicone sprays well away from the machines making paintable parts and from the paint line.

Hypothesis 2: heavy spraying

Even a silicone-free release agent causes trouble in excess. Consider this hypothesis when operators spray differently onto sticky spots such as deep ribs or bosses, when spraying is stepped up every time a part hangs up, or when an automatic nozzle leaks or its spray interval does not match the production rate. Say that on the night shift a part hung up once or twice and the operator began spraying every cycle. Runs of release agent appear down the mould face, and a hand drawn along the ribs comes away slick. When the parts are painted in the morning, the failures sit in that shift's output, and mostly around the ribs.

How much ends up on the part depends heavily on how the release agent is applied, not just on its type. Composite moulding research showed that the type of release agent and the way it is applied govern the residual contamination on the part and the effort of removing it, and that changing the application can cut that effort (Blass & Dilger, 2017). Another study observed that silicone release agent on the mould remains as small droplets rather than an even film, and noted that release agent is often over- or under-applied because the link between the amount applied and processing is poorly understood (Bainbridge et al., 2021). The more that is sprayed, the more tends to carry over to the part, and spots where droplets or runs sat can retain more, so within a single part only certain areas may peel.

Begin by matching the spray records against failures by shift. See whether failures cluster in one shift, with one operator, or right after mould maintenance or a hang-up, and sketch where paint lifted on a part to see whether it overlaps the spots where spray collects, such as ribs, bosses and deep areas. Run a wetting test on both the flat face and the rib area of the same part to see whether they differ. With automatic spraying, actually measure nozzle position, spray time, pressure and dilution and compare them with the settings.

Spray quantity belongs in the work standard, not in operator feel. Set and write down the number and length of bursts, nozzle distance and dilution in line with the release agent's TDS, and fix the nozzle position and output on automatic systems. Where parts always hang up, look for the cause on the mould side, such as draft angle, scratches on the mould face or holding pressure, rather than spraying more. After cutting the spray, log release problems alongside paint failures over the same period to find the amount that balances the two.

Hypothesis 3: under-cured coat

A semi-permanent release agent is one that, once applied, serves many cycles without reapplication. On lines using one, look at this hypothesis when paint failures appear right after mould maintenance. It applies especially when coating a cold mould in winter, when cure time is cut to meet the schedule, or when several coats are stacked in a hurry. Take a line where the mould was cleaned over the weekend and given several coats of semi-permanent release, then started straight up on Monday morning to keep to the shift start, without waiting for the film to cure. Only parts from the first few hours peel, and the failures fade on their own as the afternoon goes on.

A semi-permanent release film only performs once it has cured. A polymer dissolved in solvent is applied thin and even, the solvent evaporates, and what remains bonds chemically to the mould face as a very thin film. One product data sheet sets separate times for solvent to flash off between coats and for the final coat to cure, notes that warming the mould shortens the cure, and lists non-transferring release from the cured film as a benefit (Henkel, 2015). A PDMS-based semi-permanent film gave very effective release once cured (Critchlow et al., 2006). Before cure, much of the film is not yet bound to the mould, and since unbound chains can gather at the surface even in a fully cured silicone network (Hauer et al., 2024), it is reasonable to expect an under-cured film to hold more material that can move onto the part. As the film cures, less carries over, which also fits failures that fade with time.

The maintenance log holds the clues. Note when the release agent was applied, how many coats, the interval between coats, when production started and the mould temperature at the time, and compare them with the cure conditions in the TDS. Lay out paint failures in order of moulding time to see whether they bunch up right after maintenance and drop off later. Before start-up, rub the mould face lightly with a clean white cloth for tackiness or anything coming off, and check whether parts moulded right after maintenance and a few hours later give different wetting results.

If the cure proves short, write the coat interval and cure time from the TDS into the maintenance standard, and in cold seasons extend the time or warm the mould to cure it within the range the maker allows. The maker's data advises touching up only where release has worsened, to limit build-up of release agent (Henkel, 2015). Also set a rule that the first few shots after maintenance are held back from painting and checked with a wetting test before they move on.

Hypothesis 4: poor cleaning

If the release agent cannot be changed, whatever is left on the part must be removed before painting, and cleaning becomes the last gate. Look at this hypothesis on lines that paint without cleaning, wipe with solvent but use one cloth for too long, move cleaned parts by bare hand, or use a cleaner chosen for a different kind of soil. A cleaner works through a box of parts in turn with a single solvent-soaked cloth. The first few from the top paint well, but spot defects in the film increase towards the bottom of the box.

Cleaning works only if it suits the type of release agent left behind. The standard on preparing plastics before bonding sets out sanding and solvent wiping to remove gloss and soils such as grease and mould release, yet notes that these treatments do not necessarily give the best adhesion and may not suit industrial use as they stand (ASTM International, 2025). An institute that studies release agent residues describes first identifying the type and amount of residue by surface analysis, then choosing wet cleaning, plasma or flame treatment to suit, either removing the residue or changing it chemically so it no longer harms adhesion (Fraunhofer IFAM, n.d.). Wiping part after part with the same cloth spreads release agent lifted from one part onto the next, which is why failures grow towards the bottom of the box.

Silicone is particularly hard to remove. In tests on composites contaminated with PDMS, laser treatment did not remove the PDMS completely even at low contamination levels (Palmieri et al., 2016). Plasma and flame treatments not only strip residues but also create polar groups on the surface, giving the paint more places to hold (Awaja et al., 2009). For parts carrying silicone, then, wiping alone falls short, and adding such a treatment or keeping silicone out in the first place is the surer route.

Run a wetting test on the same part before and after cleaning to see what cleaning actually changes. Watch the real job for the type of cleaner and how often it is replaced, when the cloth is changed, the time from cleaning to painting and who handles the parts in between, and how. Compare whether failures vary with position in the box or with the operator, and whether parts cleaned twice do better than parts cleaned once.

Fixing the cleaning starts with resetting the wiping method. Wipe in one direction with a clean cloth, change it after a set number of parts, and handle cleaned parts only with clean gloves. Choose a cleaner that suits the residue, confirmed with the release agent and paint suppliers, and for parts that carry silicone, consider adding plasma or flame treatment. Whatever the method, confirm and log the cleaning result for every lot with a wetting test.

Hypothesis 5: moulding conditions

If paint began to peel after a change in moulding settings, with release agent and cleaning unchanged, look at the moulding side. Typical cases are lowering mould temperature or cutting cooling time to shorten the cycle, raising injection speed or holding pressure, and uneven mould cooling. Watch more closely with resins prone to solvent cracking, such as polycarbonate, or resins whose surface layer depends on moulding conditions, such as thermoplastic olefin, TPO, a blend of polypropylene and rubber. In the week after cooling time was cut and injection speed raised to meet output, with paint and cleaning the same, the film starts cracking or lifting only near the gate and around weld lines.

A moulded part retains stress from molecules stretched by the flow and frozen in place, and stress from cooling unevenly across thicknesses and locations; how large it is depends on moulding conditions such as mould temperature, injection speed and holding pressure (Guevara-Morales & Figueroa-López, 2014). When solvent from paint or thinner reaches a stressed part, environmental stress cracking, fine cracking at the surface with no external load, can occur. Failure analysis experience shows that moulded-in residual stress alone is often enough to cause such cracking (Cruz & Jansen, 2022). In TPO, the high shear of fast filling alters the structure near the surface, and melt temperature, mould temperature and cooling rate also affect the properties of the plastic. With such resins, an adhesion-promoting primer must wet the surface and soak into and entangle with the layer below to stick, so if the surface layer itself is weak, the paint can come away together with it (Ryntz, 2005).

Mark the peeled areas on a drawing of the part to see whether they gather at the gate, weld lines or changes in thickness. Look at the back of a lifted paint flake under a magnifier: a thin layer of plastic stuck to it means the part's surface layer broke, while a clean back means paint and surface parted. For a clear resin, set the part between two polarising sheets and look for where the rainbow fringes crowd together to judge the remaining stress. Do not skip matching the record of setting changes against the date the failures began.

Reverting the changed moulding settings and painting with the same paint for comparison is both the quickest check and the first remedy. Reset mould temperature, holding pressure and injection speed towards lower stress within the resin supplier's recommended ranges, and if needed review a post-moulding heat treatment to relieve stress with the resin supplier. On the paint side, look with the paint supplier for a paint or primer whose solvents are less aggressive to that resin.

Finding the cause

There is no need to investigate all five hypotheses at once. Start with what paperwork and a few minutes of testing can rule out. Whether the release agent contains silicone is clear from the can and the SDS, the spray and maintenance history from the records, and wetting tests can be done beside the line. Reverting moulding settings and laboratory surface analysis cost time and money, so they come later.

Next come the shape and location of the defect. Round craters dotted across the film point first to a low surface energy substance such as silicone left on the surface. Peeling that overlaps the spots where spray collects, such as ribs and bosses, points to spray quantity; failures that bunch up right after mould maintenance and then fade point to cure of the semi-permanent film; and failures that vary with position in the box or with the person cleaning point to cleaning. Paint that cracks around the gate and weld lines, with a layer of plastic on the back of the lifted film, points to moulded-in stress and the surface layer.

If shape alone does not settle it, run control trials that change one thing at a time. Change the cleaning method or add plasma treatment for only some parts of a lot, and paint parts moulded just after a thorough mould clean alongside normal parts on the same day with the same paint. Compare a shift with reduced spray against a normal shift, and put moulding settings back to their earlier values once. Change only one thing at a time, or there is no telling which change worked.

Judge whether the job is done by adhesion measured the same way each time. Run a cross-cut test, which cuts a lattice into the film and grades how much comes away (ISO, 2020), or a tape test, which applies and pulls tape over cuts, under the same conditions and on the same number of parts as before the change (ASTM International, 2023b). Check printing with the rub or tape test in the customer's specification. The cause has been removed only once the failure rate has stayed at its normal level over several lots.

The hypotheses can overlap. Moulding conditions that make parts hard to eject lead to more spraying, spray over an under-cured semi-permanent film leaves two residues at once, and the more that is left, the less a given cleaning can remove. In such cases, put the type, amount and film condition of the release agent right first, then look again at cleaning and moulding conditions, because while release agent remains on the surface, the effect of changing cleaning or moulding cannot be compared fairly.

Limits and cautions

Surface treatment criteria, wetting tension targets, release agent coat intervals and cure times, and suitable moulding settings differ by resin, paint, ink and release agent, so numeric decisions follow each product's TDS and the suppliers' guidance. The cross-cut test does not measure adhesion as such, so where a numerical adhesion strength is needed, use a separately specified method such as a pull-off test (ISO, 2020). Parts with set specifications, such as automotive exterior parts, are judged by the customer's specified tests, and surface composition analysis and residual stress judgements belong to the laboratory.

Safety matters too. Use spray release agents and cleaning solvents with the ventilation and protective equipment set out in each product's SDS, and since they may be flammable, use and store them away from flames and hot surfaces. Apply semi-permanent release or clean a mould only with the machine stopped and locked out, and wear gloves against hot mould faces. Plasma and flame treatment equipment should be run only by trained staff under set conditions.

Sources

  1. ASTM International. (2023a). ASTM D2578-23, Standard test method for wetting tension of polyethylene and polypropylene films. https://store.astm.org/d2578-23.html
  2. ASTM International. (2023b). ASTM D3359-23, Standard test methods for rating adhesion by tape test. https://store.astm.org/d3359-23.html
  3. ASTM International. (2025). ASTM D2093-03(2025), Standard practice for preparation of surfaces of plastics prior to adhesive bonding. https://store.astm.org/d2093-03r25.html
  4. Awaja, F., Gilbert, M., Kelly, G., Fox, B., & Pigram, P. J. (2009). Adhesion of polymers. Progress in Polymer Science, 34(9), 948–968. https://doi.org/10.1016/j.progpolymsci.2009.04.007
  5. Bainbridge, K., Schoenholz, C., & Zobeiry, N. (2021). Investigating the aging of release coating in aerospace composites manufacturing. Undergraduate Research in MSE, 2. https://doi.org/10.6069/ssywg443
  6. Blass, D., & Dilger, K. (2017). CFRP-part quality as the result of release agent application – Demoldability, contamination level, bondability. Procedia CIRP, 66, 33–38. https://doi.org/10.1016/j.procir.2017.03.219
  7. Blass, D., Hartwig, S., & Dilger, K. (2017). A qualitative, process-parameter-based model for the release agent transfer during CFRP-part production: An approach to increase the initial bondability. Applied Adhesion Science, 5, 16. https://doi.org/10.1186/s40563-017-0095-7
  8. Critchlow, G. W., Litchfield, R. E., Sutherland, I., Grandy, D. B., & Wilson, S. (2006). A review and comparative study of release coatings for optimised abhesion in resin transfer moulding applications. International Journal of Adhesion and Adhesives, 26(8), 577–599. https://doi.org/10.1016/j.ijadhadh.2005.09.003
  9. Cruz, J. C., & Jansen, J. A. (2022). Environmental stress cracking. In T. J. Menna (Ed.), ASM handbook: Vol. 11B. Characterization and failure analysis of plastics. ASM International. https://doi.org/10.31399/asm.hb.v11B.a0006917
  10. Fraunhofer IFAM. (n.d.). Fighting release agent residues – for successful downstream processing of components. Fraunhofer Institute for Manufacturing Technology and Advanced Materials. Retrieved November 2026. https://www.ifam.fraunhofer.de/en/technologies/fighting-release-agent-residues.html
  11. Guevara-Morales, A., & Figueroa-López, U. (2014). Residual stresses in injection molded products. Journal of Materials Science, 49(13), 4399–4415. https://doi.org/10.1007/s10853-014-8170-y
  12. Hauer, L., Naga, A., Badr, R. G. M., Pham, J. T., Wong, W. S. Y., & Vollmer, D. (2024). Wetting on silicone surfaces. Soft Matter, 20(27), 5273–5295. https://doi.org/10.1039/d4sm00346b
  13. Henkel. (2015). Technical data sheet: LOCTITE FREKOTE 44-NC. Henkel Corporation.
  14. International Organization for Standardization [ISO]. (2020). ISO 2409:2020, Paints and varnishes — Cross-cut test. https://www.iso.org/standard/76041.html
  15. Palmieri, F., Ledesma, R., Cataldo, D., Lin, Y., Wohl, C., Gupta, M., & Connell, J. (2016). Controlled contamination of epoxy composites with PDMS and removal by laser ablation. Paper presented at SAMPE Long Beach 2016, NASA Technical Reports Server. https://ntrs.nasa.gov/citations/20160009092
  16. Ryntz, R. A. (2005, July). Real world performance of painted plastic components. JCT CoatingsTech, 30–36. https://www.paint.org/wp-content/uploads/2021/12/Real-World-Performance-of-Painted-Plastic-Components.pdf

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.