Looking for a product with more extreme pressure additive, or running a stronger mix, is the usual response when stainless machining gets harder after chlorinated coolant is dropped, but chlorinated additives often cannot be replaced by any single other additive, so simply adding more may leave the gap open. What actually lies behind it can be extreme pressure additives that work at different temperatures, a changed base oil and viscosity, too little polar additive, fluid that never reaches the cutting edge, or a tool unsuited to stainless, and sometimes two or more at once.

Background

A few weeks after a cutting fluid with chlorinated extreme pressure additive is replaced by a chlorine-free product, complaints pile up in the cell that handles stainless parts. Taps snap in the hole, drills and reamers dull faster than before, and work material sticks to the cutting edge and tears the surface. Carbon steel parts come off as they always did, so the problem seems to sit where stainless meets the new fluid.

A broken tap stuck inside a part usually means scrapping that part, and more frequent tool changes mean more machine stoppage. Going back to the old product is not easy either. Short-chain chlorinated paraffins have already been restricted or banned in the U.S., Canada and the European Union (Canter, 2014), and in 2025 medium-chain chlorinated paraffins were also listed for elimination under the Stockholm Convention. Metalworking fluids keep only an exemption that may run until 2036 at the latest, for heavy-duty processes in professional or industrial settings with collection systems (UN, 2025).

Stainless steel, austenitic grades in particular, ranks among the hardest alloy steels to cut. The cutting zone hardens as it is worked, heat escapes poorly, and built-up edge, work material sticking to the edge, forms readily (Kaladhar et al., 2012). In such severe contact, extreme pressure additives react with the metal surface to form chemical films such as iron chlorides, iron phosphides and iron sulphides, and these films reduce friction, wear and scoring and prevent welding (Canter, 2007). Because chlorinated additives do several jobs at once, they often cannot be replaced by one additive type alone, and alternative products are built from combinations of additives that suit the application (Canter, 2014).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: lay the technical data sheets, the TDS, of the old and new products side by side to compare extreme pressure additive type, viscosity and recommended concentration, and record which operations got worse after the switch, together with tool, speed and fluid delivery.

Hypothesis 1: EP temperature gap

This hypothesis usually shows itself in slow, heavily loaded work: tapping, reaming, broaching, thread cutting and small-diameter drilling, where the edge pushes slowly through the material. Pay closer attention if high-speed turning on the same machine is fine and only taps and reamers have got worse. A cell cutting internal threads in 304 stainless blocks is a case in point. Tap and speed are the same as before, yet tap life has dropped noticeably since the switch, and a thin smear of silvery stainless is stuck between the teeth of the taps pulled out.

Extreme pressure additives do not work at just any temperature. A film forms only when they react with the metal surface, and the temperature range for that reaction differs by type. According to an industry review, polar lubricity additives work from ambient up to about 200 °C, chlorinated additives at about 180 to 420 °C, phosphorus types higher, and sulphur types higher still, in a range that reaches about 1,000 °C (Canter, 2007). The same review explains that in less severe operations the temperature at the cutting point may not rise enough to activate an additive, and that a tool can fail before the extreme pressure additive comes into play, so a boundary lubricity additive is needed to cover that gap. The research literature describes the same frame, with extreme pressure and antiwear additives building protective films by chemical reaction at the rubbing surfaces (Li et al., 2022). Chlorinated additives covered the lower range broadly, so a substitute built mainly on sulphur, used for slow tapping, can leave a stretch without a protective film until the edge gets hot enough for sulphur to react. In that stretch stainless welds onto the edge, and when the built-up edge breaks away it can tear the edge with it.

Begin by listing which operations got worse. If problems cluster in slow work such as tapping, reaming and broaching while high-speed work is fine, this hypothesis gains weight. Examine the tools pulled out under a magnifier for work material welded to the edge, and confirm from the new product's TDS or the supplier's information whether its extreme pressure additive is sulphur-based and whether it also carries phosphorus or polar additives. The difference between the two products can be put into numbers with a tapping torque test, which compares the torque measured with the same tap in each fluid (ASTM International, 2025).

If slow work seems to be left without a protective film, the right move is to find with the supplier a combination of additives with overlapping temperature ranges, not to add more of one extreme pressure additive. Alternative additives are used in synergistic combinations that suit the application, and the industry reports that they have replaced chlorinated additives in drilling, milling and turning of stainless and highly alloyed steels (Canter, 2014). If only a particularly severe operation such as tapping is affected, a product matched to that operation alone is another option. Either way, run a torque test with the same tap before switching and compare it with the old product.

Hypothesis 2: different base oil

If removing chlorine also meant changing supplier or product family, the base oil has very likely changed too: from mineral oil to a synthetic or ester base oil, or to a product of a different viscosity grade. Dab the new product on a finger and it may feel thinner than the old one and run off quickly, and the oil film left on a drill just pulled out may look thinner as well. Operators may also say the cut sounds sharper.

Base oil is the body that dissolves the additives and carries them to the edge. Solubility in base stocks is one of the factors to weigh when choosing an extreme pressure additive (Canter, 2007), because the same additive can behave differently depending on the base oil it is dissolved in. In form tapping tests that kept the additive package fixed and changed only viscosity, torque did not change, but the interaction between base oil and a sulphur additive changed efficiency markedly (Bierla et al., 2008). So the viscosity figure alone says little, and the question is whether the base oil type and the additives in it changed together. Kinematic viscosity is measured by a standard test method at a set temperature such as 40 °C (ASTM International, 2024), so the figures in the two TDS can be compared on the same basis.

Copy the 40 °C kinematic viscosity and base oil type from both TDS, and measure the viscosity of the oil in service in the machine against the fresh oil, since hydraulic oil or lubricant that leaked in during use may have changed its viscosity and make-up. The surest way to settle this hypothesis is to obtain products from the same additive family that differ only in viscosity or base oil and run a torque test on each with the same tap.

What needs attention here is the pairing of base oil and additives. If the torque test shows large differences between base oils, ask the supplier for a product built on a base oil that suits the additive, or one of another viscosity grade. If other oil has mixed in and changed the viscosity, stop the leak and replace or top up the oil. When raising viscosity, watch the amount carried off on chips and the load on filters as well.

Hypothesis 3: low polar additive

Look at this hypothesis when the new product carries less fatty or ester material than the old one, or, for a water-miscible fluid, when it has moved to a semi-synthetic with less oil. It shows especially in work where the edge stays too cool for extreme pressure additives to act: reaming, tapping and finishing. In one cell, stainless holes are finished with a reamer, and since the switch the bore surface has shown torn texture while a thin metal layer coats the reamer edge. Chips also run longer and tougher than before.

A polar additive has one end of the molecule that clings to the metal surface and another that mixes with the oil, so it builds a thin film on the metal and reduces metal-to-metal contact. The classic example is an ester, added as a natural oil such as canola or lard oil or as a synthetic ester (Canter, 2007). This film is what protects the edge at the low temperatures before extreme pressure additives react, so its role grows in a product without chlorine. In tests drilling AISI 316L stainless steel, all five vegetable-based cutting fluids outperformed the mineral oil reference, and the best raised tool life by 177% and cut thrust force by 7% (Belluco & De Chiffre, 2004). High molecular weight esters are also listed among alternatives to chlorinated additives (Canter, 2014).

The amount of polar additive may not appear in full on the SDS, so ask the supplier directly. On the floor, a quick route is to compare drill thrust or spindle load with the old and new products. In the same study, cutting forces agreed well with tool life and were more repeatable, so the authors suggested them as an evaluation method that costs less time and money than tool life testing (Belluco & De Chiffre, 2004). Record torn texture on finished surfaces, chip shape and any welded layer on the reamer edge as well.

If thrust or torque is clearly higher with the new product and finished surfaces tear, trial with the supplier a grade carrying more polar additive or an ester-based product. For a water-miscible product, also consider a grade with more oil or a higher concentration within the recommended range. Measure the replacement again by thrust or tapping torque with the same tool and conditions to confirm it has returned to the old level.

Hypothesis 4: poor fluid delivery

Fluid delivery sometimes changes along with the fluid: a move from flood to minimum quantity lubrication, MQL, a tidy-up of nozzles, or work on pumps and filters. Cases where tool length changed but the nozzles did not, or where deep holes are drilled without through-tool coolant, also belong here. Watch a drill cutting a deep hole, and the fluid from the nozzle wets only the tool shank and bounces off the hole entrance. The chips coming out are tinged blue at the ends.

Additives work only if they reach the contact at the cutting edge. Extreme pressure additives react with the metal surface and polar additives cling to it to form a film (Canter, 2007), so with the same fluid, less of it reaching the edge means less effect. Austenitic stainless has much lower thermal conductivity than structural carbon steels, so heat concentrates where chip and tool meet (Endrino et al., 2006). Supply pressure matters too. In turning nickel-base alloy 718 with coated carbide, a 203 bar supply raised tool life by up to 740% over conventional flood, which the authors put down to the jet lifting the chip and getting fluid closer to the cutting zone (Ezugwu & Bonney, 2004).

Watch where the fluid lands with the machine running. Check that nozzles point at the edge and at where chips leave, and that they are reset at every tool change, and look at pump delivery pressure and flow and at blocked nozzles or filters. For MQL, measure whether the set oil quantity is really delivered. Chip colour and heat tint on the tool are signs of heat build-up, so compare them before and after the delivery change.

With the cause narrowed to delivery, getting fluid to the edge comes first. Re-aim the nozzles at the edge and under the chip, and for deep holes and tapping, trial through-tool coolant or higher pressure. Conventional machining relies heavily on cutting fluid to lower cutting temperatures and forces, and one review sees great potential for MQL as a substitute for flood (Boswell et al., 2017). Changing the method, though, changes both the amount and the make-up of fluid reaching the edge, which mixes the fluid's effect with the delivery's. So if the trouble began after a move to MQL, do not test the chlorine-free fluid and MQL together; check the new fluid on its own under flood first. Only then can the next step show whether MQL suits that operation.

Hypothesis 5: unsuited tool

Suspect this hypothesis in cells that cut carbon steel and stainless with the same tools, with general-purpose tools whose edges are honed blunt, with uncoated high-speed steel taps, and with tools whose geometry changed in regrinding. While chlorinated fluid was in use, generous lubrication may have hidden a tool's shortcomings, and the gap may have surfaced after the switch. Suppose a cell uses the end mills from its carbon steel parts on stainless parts too. Edges that had no trouble in carbon steel dull quickly in stainless, with lumps of work material building on the edge and breaking off again and again.

Austenitic stainless is highly plastic and work-hardens readily, which tends to make cutting conditions severe. In end milling tests on this material, a nano-crystalline AlTiN coating wore least among four hard, high-aluminium PVD coatings, and the authors recommended hard coatings with low thermal conductivity and a smooth surface (Endrino et al., 2006). How built-up edge forms and breaks away depends on material, tool coating and friction, and when it breaks away it can pull tool material with it and speed up wear (Fox-Rabinovich et al., 2020). Geometry changes the outcome as well. In a study that optimised the helix angle, chamfer angle and relief of spiral taps made for 304 stainless by finite element simulation, the resulting taps cut the average maximum axial force by 33.22% and the average maximum torque by 13.41% in real tapping tests (Pi et al., 2025).

Pull the tool and inspect the edge under a magnifier. Note welded work material, small chips in the edge, spots where the coating has worn through and notch wear, and confirm whether the tool is one the tool maker recommends for stainless and whether its geometry after regrinding matches the original. Trial one tool recommended for stainless with the new fluid, and see whether changing only the tool, with the same fluid, changes the result.

If the evidence leans towards the tool, choose stainless coatings and geometry with the tool maker and keep separate tools for carbon steel and stainless. Use taps with geometry and coatings made for stainless, and send regrinding only to shops that can reproduce the original geometry. In tests tapping stainless steel, the depth cut in each pass changed both cutting torque and tap life (Uzun & Korkut, 2016), so set tapping conditions within the tool maker's recommended range too. After the tool change, log tool life for a while before changing the fluid again, so any remaining problem can be traced separately to the fluid.

Finding the cause

Start with what is easy to check. Comparing the two TDS, nozzle aim and flow, and looking at the tool edge can all be done without a long stop. Tapping torque tests and thrust measurements need test pieces and equipment, so they come next.

Which operations got worse is the first fork. If trouble clusters in slow tapping, reaming and broaching, look first at the additive temperature range and the polar additive; if it appears only in deep holes or at certain tool positions, look at delivery; and if carbon steel cut with the same tools is fine while only stainless suffers, look at the tool. If the supplier changed altogether, the base oil may have changed too, so keep that possibility open.

Next comes a control test that separates the fluid from everything else. Measuring torque with the same tap, test piece and speed in the old and new products shows the difference in the fluids themselves. A standard test method measures relative torque between a test fluid and a reference fluid, so this comparison can follow a set procedure (ASTM International, 2025). If the torque difference is small but the floor is still struggling, turn to delivery or the tool.

Once a remedy is chosen, finish with a final check. Count tool life, tap breakages and finished surface condition over a period on the same basis as before the change, and call it done when they are back to the old level. Change only one thing at a time, or there is no record of which one worked.

The hypotheses can overlap. A new chlorine-free product changes extreme pressure additive, base oil and polar additive as one package, so causes on the additive temperature range, base oil and polar additive side tend to arrive together, and if a move to MQL or a tool rationalisation lands at the same time, the causes tangle further. In such cases return delivery and tooling to the old conditions and hold them there, then test the fluid, because while delivery and tooling keep changing, the effect of a fluid change cannot be compared fairly.

Limits and cautions

Additive combination, viscosity, recommended concentration, supply pressure, tool geometry and cutting conditions differ by material, operation, machine and product, so numeric decisions follow the fluid's TDS and the tool maker's guidance. Rules and exemptions for chlorinated paraffins differ by country and are still changing, so check national regulations before going back to an old product. Sulphurised extreme pressure additives can stain copper alloys to some extent (Canter, 2007), so if brass or bronze parts are cut with the same oil, test that effect as well.

Safety matters too. For both the new and the old product, follow the safety data sheet, the SDS, for gloves and eye protection, and since raising supply pressure can increase mist, check machine guarding and mist extraction. Metalworking fluids can cause dermatitis through skin contact and respiratory disease through breathing in mist (HSE, 2024). Keep waste oil drained from chlorinated products separate and dispose of it under local rules.

Sources

  1. ASTM International. (2024). ASTM D445-24, Standard test method for kinematic viscosity of transparent and opaque liquids (and calculation of dynamic viscosity). https://store.astm.org/d0445-24.html
  2. ASTM International. (2025). ASTM D8288-25, Standard test method for comparison of metalworking fluids using a tapping torque test machine. https://store.astm.org/d8288-25.html
  3. Belluco, W., & De Chiffre, L. (2004). Performance evaluation of vegetable-based oils in drilling austenitic stainless steel. Journal of Materials Processing Technology, 148(2), 171–176. https://doi.org/10.1016/S0924-0136(03)00679-4
  4. Bierla, A., Fromentin, G., Martin, J. M., Le Mogne, T., Minfray, C., & Genet, N. (2008). Evaluation of lubricant viscosity and base oil effects by form tapping test [Conference paper]. HAL. https://hal.science/hal-00910301
  5. Boswell, B., Islam, M. N., Davies, I. J., Ginting, Y. R., & Ong, A. K. (2017). A review identifying the effectiveness of minimum quantity lubrication (MQL) during conventional machining. The International Journal of Advanced Manufacturing Technology, 92(1–4), 321–340. https://doi.org/10.1007/s00170-017-0142-3
  6. Canter, N. (2007, September). Special report: Trends in extreme pressure additives. Tribology & Lubrication Technology, 10–17. https://www.stle.org/images/pdf/STLE_ORG/BOK/OM_OA/Additives/Trends%20in%20Extreme%20Pressure%20Additives_tlt%20article_Sept07.pdf
  7. Canter, N. (2014, September). EP additives: Regulatory updates of chlorinated paraffins and options on alternatives. Tribology & Lubrication Technology. https://www.stle.org/files/TLTArchives/2014/09_September/Tech_Beat.aspx
  8. Endrino, J. L., Fox-Rabinovich, G. S., & Gey, C. (2006). Hard AlTiN, AlCrN PVD coatings for machining of austenitic stainless steel. Surface and Coatings Technology. https://doi.org/10.1016/j.surfcoat.2005.10.030
  9. Ezugwu, E. O., & Bonney, J. (2004). Effect of high-pressure coolant supply when machining nickel-base, Inconel 718, alloy with coated carbide tools. Journal of Materials Processing Technology, 153–154, 1045–1050. https://doi.org/10.1016/j.jmatprotec.2004.04.329
  10. Fox-Rabinovich, G., Gershman, I., Yamamoto, K., Dosbaeva, J., & Veldhuis, S. (2020). Effect of the adaptive response on the wear behavior of PVD and CVD coated cutting tools during machining with built up edge formation. Nanomaterials, 10(12), 2489. https://doi.org/10.3390/nano10122489
  11. Health and Safety Executive [HSE]. (2024). Ill health from metalworking and water-mix wash fluids and what to do about it. Updated 2024. https://www.hse.gov.uk/metalworking/waterillhealth.htm
  12. Kaladhar, M., Subbaiah, K. V., & Rao, C. H. S. (2012). Machining of austenitic stainless steels – A review. International Journal of Machining and Machinability of Materials, 12(1/2). https://doi.org/10.1504/IJMMM.2012.048564
  13. Li, H., Zhang, Y., Li, C., Zhou, Z., Nie, X., Chen, Y., Cao, H., Liu, B., & Zhang, N. (2022). Extreme pressure and antiwear additives for lubricant: Academic insights and perspectives. The International Journal of Advanced Manufacturing Technology, 120(1–2). https://doi.org/10.1007/s00170-021-08614-x
  14. Pi, J., Zhang, W., & Yang, H. (2025). Optimization of structural parameters for 304 stainless steel specific spiral taps based on finite element simulation. Machines, 13(8), 655. https://doi.org/10.3390/machines13080655
  15. United Nations [UN]. (2025). Stockholm Convention on Persistent Organic Pollutants: Amendments to Annex A (Depositary notification C.N.672.2025.TREATIES-XXVII.15, decision SC-12/10 listing medium-chain chlorinated paraffins). https://treaties.un.org/doc/Publication/CN/2025/CN.672.2025-Eng.pdf
  16. Uzun, G., & Korkut, I. (2016). The effects of cutting conditions on the cutting torque and tool life in the tapping process for AISI 304 stainless steel. Materiali in Tehnologije, 50(2), 275–280. https://doi.org/10.17222/mit.2015.044

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.