KALTECKOREA

BlogApplication notes

Why does coolant on magnesium machining lines wear out so fast?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Metalworking Fluids (MWF)

Adding more concentrate or dumping the whole sump is the usual response when coolant on a magnesium line goes off quickly, but if the cause stays, the fresh fluid goes the same way. What actually lies behind it can be hardness built up by dissolved magnesium ions, pH pushed up by magnesium hydroxide, release agent carried in on castings, magnesium soap scum, hard make-up water or fines left in the fluid, and sometimes two or more at once.

Background

On a line machining magnesium die castings, the water-miscible coolant is changed, and within a few weeks it is due again. White crust builds on nozzles and pipes, filters block quickly, an oil layer floats on the tank and the fluid separates like cream. Compared with steel or aluminium lines on the same coolant, the change interval is strikingly short.

Every change costs concentrate and waste disposal and stops the line. Blocked nozzles cut cooling and chip flushing, which hits tool life and surface finish at once, and on magnesium it becomes a safety issue as well. Chips that pile up inside the machine add fuel for a fire, so magnesium machining guidance requires chips to be flushed away with plenty of coolant and the supply flow to be monitored (DGUV, 2020).

Water-miscible coolant is used on magnesium to prevent fires and extend tool life. A report from one plant that moved from dry machining to water-miscible coolant listed these benefits, along with problems to solve: fluid splitting, hydrogen generation and salt deposits on tools and machines (Spicer et al., 1991). The root lies in magnesium reacting with water to form magnesium hydroxide and hydrogen (Song & Atrens, 1999). During machining, metal dissolves little by little into the fluid, and that changes the chemistry of the coolant.

In such cases the technical team sets up the six hypotheses below and rules them out one by one. The start is always the same: measure the concentration, pH and hardness of the tank fluid and the hardness of the make-up water, and compare them with the ranges in the coolant's technical data sheet, the TDS, and with the values on the day the tank was filled.

Hypothesis 1: magnesium hardness

Dissolved magnesium builds up with the amount machined, so it shows first in small stand-alone tanks rather than large central systems, and on lines where the fluid is only topped up and never dumped. Picture a cell where one machining centre with its own small tank cuts magnesium gearbox housings all day. For the first few days after a change the fluid runs clear, then after a few weeks white crust forms at the nozzle tips and a hard layer starts to settle on the tank walls. The steel cell next door, on the same concentrate, shows no such layer.

Dissolved magnesium stays in the fluid as ions. Water leaves by evaporation, but ions stay behind, so hardness climbs the longer machining goes on. Nothing breaks them down, so they rarely fall unless fluid is dumped or diluted. A study of semi-synthetic coolants reported that divalent ions such as calcium and magnesium accumulate over time from hard top-up water and from metal workpieces and break down the emulsion, and added that EDTA, dosed to tie up hardness ions, can be ineffective or very inefficient because it interacts directly with the emulsifiers (Zimmerman et al., 2004). German accident insurance guidance for magnesium calls this a rise in hardness and notes that glass-hard layers can block pumps and pipes and seriously cut the coolant supply (DGUV, 2020).

Hardness can be read on the spot with test strips, and for figures to keep, run the EDTA titration for calcium plus magnesium together with the titration for calcium alone (ISO, 1984a; ISO, 1984b). The difference is the magnesium share. If total hardness in the tank is far above that of the make-up water and its magnesium share rises with the amount machined, the hardness comes from the workpieces rather than the water. Measuring on the same day each week and plotting the trend since the last change shows how fast it is rising.

Once build-up is confirmed, slowing the magnesium input comes first. Magnesium machining guidance recommends steady filtration of magnesium particles with filter fleece or a pressure belt filter to reduce or delay ions dissolving and building up, and regular hardness checks so action is taken early (DGUV, 2020). Before adding more hardness stabiliser, confirm with the supplier whether the concentrate is built to tolerate hardness for magnesium work, and agree a hardness level at which part of the fluid is replaced.

Hypothesis 2: pH pushed up

Suspect pH where chips and fluid stand together after machining stops: under the chip conveyor, in chip bins, in tanks idle over the weekend. The longer chips soak, the longer they have to react. At the first check on a Monday morning, the pH meter reads higher than on Friday, and a thin layer of white, powdery sediment lies on the tank floor. As the shift changes, a few operators say the backs of their hands sting.

The route to a higher pH is in the reaction. As magnesium dissolves, magnesium ions form at the metal while, at other sites, water breaks down into hydrogen gas and hydroxide ions, and the two combine into magnesium hydroxide, which barely dissolves in water (Song & Atrens, 1999). Hydroxide is alkaline, so as the reaction continues it pushes the fluid towards the alkaline side. Diluted water-miscible coolant usually sits between pH 8.5 and 9.5, held there by buffering components, but above 9.5 it is treated as a value to control because of skin reactions (Khan et al., 2021). That metalworking fluids can cause dermatitis and respiratory illness is set out in exposure criteria as well (NIOSH, 1998).

Measure pH at the same time and place every week; the guidance also calls for regular checks, such as weekly, of pH, concentration and nitrite in water-miscible coolants (DGUV, 2020). A pH meter catches small shifts better than strips. Record values during running and after long stops side by side, and if the rise after a stop is large, look at standing chips and fluid. Measure the pH of fluid standing in chip bins as well, and see whether the white sediment on the tank floor has grown.

If high pH looks rooted in magnesium, cut the time chips sit in fluid rather than simply bringing the number down with acid or additives. Drain fluid from chip bins, and clear chips from the conveyor and tank corners before the weekend. The same guidance recommends coolants with inhibitor additives that greatly reduce hydrogen formation (DGUV, 2020), so check with the supplier whether the formulation slows the magnesium reaction. While pH is high, keep gloves and skin protection in use.

Hypothesis 3: release agent carry-in

This hypothesis starts with the part, not the tank. Watch for it where castings go straight from the die-casting cell to machining without washing, after the casting side changes release agent type or spray volume, and on parts with many deep pockets and ribs. Suppose that from the month after the caster changed release agent, the oil layer on the tank thickened and the skimmer began removing noticeably more. On the machining side, neither the concentrate nor the process has changed.

Die-casting release agents are often wax dispersed in water as an emulsion; some use mineral, synthetic or ester oils or polysiloxanes, and they contain additives that keep the organic ingredients stably mixed in water. Wax-based release agents are known to leave deposits (NürnbergMesse, 2020). These components left on the casting can be washed into the coolant during machining, and from then on they take the same path as oil leaking from the machine. A coolant containing emulsifiers takes in foreign oil for a while, but once the emulsifiers are saturated the oil floats, and the floating oil binds with fine particles into sludge that gives bacteria that shun oxygen a good place to grow (Khan et al., 2021).

Start by wiping the castings. Wipe a few parts before machining with a clean white cloth or one wetted with solvent, see whether wax or oil comes off, and compare with parts that have been washed. At the tank, log the oil layer thickness and the skimmer's take with dates, and line them up against changes on the casting side. A rule of thumb holds that oil covering the whole tank surface means foreign oil above 2% of the total fluid, enough to harm coolant life if left alone (Khan et al., 2021).

If release agent is the cause, the fix needs the casting side. Get the release agent's SDS and spray settings, check what changed, and decide whether spray volume can come down or a washing step should go in before machining. On the machining side, remove floating oil steadily with a skimmer or a centrifuge, and check concentration and pH more often while the oil is coming in.

Hypothesis 4: magnesium soap scum

It tends to appear in emulsions and semi-synthetic coolants that rely heavily on anionic emulsifiers to disperse oil in water, after hardness has already risen. Filter bags come out smeared with a sticky grey paste, and a slimy film settles inside nozzles and around the edge of the tank surface. From around then, even with concentrate added as usual, the fluid loses its milky look and seems thin, and oil separates on top of a sample bottle left standing overnight.

Soap scum forms where hardness meets emulsifier. Negatively charged emulsifiers such as fatty acid soaps bind divalent ions such as magnesium into metal soaps that do not dissolve in water, and magnesium machining guidance calls these solid magnesium soaps and treats them as deposits that block pipes and pumps (DGUV, 2020). As emulsifier is lost this way, less is left to coat the oil droplets, so the droplets grow and oil and water finally separate. A study that designed hard-water-stable semi-synthetic coolants used mixed anionic and nonionic emulsifier systems and reported stable particle size in hard water when the molar ratio of oil to total emulsifier was 0.5 or less (Zimmerman et al., 2003).

The check begins at filters and nozzles. Rub the trapped residue between the fingers to tell gritty metal particles from sticky soap paste, and send it for analysis if needed. Stand tank fluid in a clear bottle for a day and see whether oil separates on top or a cream layer forms. A bottle of the same concentrate freshly mixed in soft water alongside makes the comparison easy. Put the hardness trend next to this, and it shows whether the rise in hardness and the growth of scum line up in time.

Clear out a system where scum has built up first. Remove deposits from nozzles, pipes and tank walls and change the filters, then work on what lowers hardness as well: filtration of magnesium particles and control of make-up water. If the concentrate is a hardness-sensitive formulation, review with the supplier a change to one whose emulsifiers are designed to tolerate hard water and magnesium hardness. Once soap scum has formed, the lost emulsifier is hard to bring back, so if separation is clear, replacing the fluid is the better choice.

Hypothesis 5: hard make-up water

Look at the make-up water first in summer when much water is lost, in plants topping up with groundwater, and after a change of water source. A typical case is a line where the tank level drops visibly every shift and operators top up from a tap hose just to restore the level. On a midsummer afternoon the level alarm sounds, and an operator hangs a hose in the tank and goes off to another job. No concentrate goes in, and this happens several times a day.

Evaporation takes only water. The calcium and magnesium dissolved in it stay in the tank, and each top-up brings fresh hardness in, so hardness builds in step with the volume of water added. That is why the study above names hard top-up water among the routes by which divalent ions accumulate (Zimmerman et al., 2004). A hardness of 80 to 125 ppm as calcium carbonate is given for water used to dilute coolant; harder water invites chemical instability, emulsion splitting and scum formed with the emulsifiers, while overly soft water invites foam (Khan et al., 2021). On a magnesium line, magnesium dissolved from the work adds to this, so the same make-up water leaves less margin than on a steel line.

Measure the make-up water and the tank side by side. Test the total and calcium hardness of the make-up water by the same methods used for the tank (ISO, 1984a; ISO, 1984b), and log daily top-up volume from a water meter or the tank level record. If calcium hardness in the tank rises with top-up volume, the water is the source; if calcium holds steady and only magnesium climbs, the work is. Check the records, too, for large seasonal swings in top-up volume.

If the make-up water is the source, changing the water is the most direct fix. Water stripped of minerals by reverse osmosis or deionisation largely shuts off the route by which hardness comes in with the water and can extend coolant life (Khan et al., 2021). Magnesium dissolving from the work is unchanged, so keep measuring hardness. Restore the level with dilute premix rather than plain water so concentration holds steady, and if foam increases with very soft water, agree an antifoam approach with the supplier.

Hypothesis 6: fines left in the fluid

Suspect fines in processes that throw off short, thin chips and powder, such as high-speed milling, drilling and tapping, in tanks filtered by little more than a chip basket, and in tanks with many corners where chips settle. At a scheduled shutdown the tank is emptied: a thick layer of grey sludge covers the floor, and small bubbles rise when it is turned with a shovel. If that floor was left in place at the last change, the fresh fluid began life sitting on this sludge.

The finer the chips, the larger the surface touching water. Fine magnesium particles react with water or moisture, giving off hydrogen and heat, and the guidance warns that wet sludge can heat itself to ignition and that hydrogen mixed with air can form an explosive mixture (DGUV, 2020). Hydrogen in air above 4 vol% can be ignited by a spark or static discharge, though in the same study's measurements the amounts generated in typical processes were relatively small (Tomac et al., 1996). From the coolant's side, the particles left behind release magnesium ions as they react, raising hardness; they ride the pump back to the cut and wear tools like an abrasive; and they bind with floating oil into sludge where bacteria thrive (Khan et al., 2021).

The tank floor says the most. Check sludge depth in the tank and under the chip conveyor at regular intervals, and draw a set volume of fluid, filter it through paper and weigh the dried solids to see in numbers whether filtration is keeping up. If shiny particles still show in fluid past the filter, the filter grade is too coarse for the process. Look at chip heaps inside the machine and around drains too, and confirm that extraction runs in enclosed spaces where hydrogen could gather.

Fines call for better filtration and removal. The guidance calls for flushing chips away with ample coolant, adding wash nozzles inside the machine so chips do not pile up, and running extraction so mist and hydrogen do not collect. Filter fleece loaded with magnesium fines is a reactive fire load, so remove it from the work area regularly and keep it in non-combustible, lidded, vented containers (DGUV, 2020). Collect, store and handle fine metal powder to the requirements of the combustible metals standard (NFPA, 2022). When the tank is changed, remove the floor sludge too, or the fresh fluid will not last.

Finding the cause

Six hypotheses need not be investigated all at once. Rule out first what test strips and meters settle in a few minutes. Concentration, pH, tank and make-up water hardness, oil layer thickness and floor sludge can all be checked without stopping the line. What needs another department or a laboratory, such as casting surfaces, release agent data and residue analysis, comes after.

The first fork is where the hardness came from. If tank hardness is far above the make-up water, the difference is mostly magnesium and it rises with output, look at ions dissolved from the work and at fines left in the fluid. If calcium climbs as well and moves with top-up volume and season, look at the make-up water. If hardness holds steady but the oil layer thickens, the source is release agent carried in on castings or oil leaking from the machine.

Next is the look of the fluid and the residue. Hard white crust on nozzles and walls points to hardness and magnesium hydroxide, while sticky grey paste blocking filters, with the fluid separating, suggests emulsifier lost as soap. A large pH rise after a long stop points to chips left standing, and thick sludge with bubbles rising from it points to fines that escaped filtration.

If that still does not settle it, run beaker control tests. Mix the same concentrate in soft water and in the plant's make-up water, two beakers of each, add magnesium chips to one beaker of each pair, and measure hardness, pH and separation over several days; this separates the water's share from magnesium's. On the floor, machine washed and unwashed castings separately, or tighten filtration by one step, changing only one thing at a time. Afterwards, compare the days from one fluid change to the next and the rate of hardness rise on the same basis, and the job is done only when those figures improve.

The hypotheses are tangled together. Fines left in the fluid release magnesium ions that raise hardness, built-up hardness ties emulsifier into soap and removes it (DGUV, 2020), and hard make-up water adds calcium and magnesium on top. So when several signs appear together, put filtration, chip removal and make-up water right first, restart with fresh fluid in a tank cleaned down to the floor, and watch the hardness and pH trends. Change the concentrate while magnesium input is still unchecked, and there is no telling what made the difference.

Limits and cautions

Control ranges for concentration, pH and hardness, and the point at which to change the fluid, differ by concentrate and process, so numeric decisions follow the product's TDS and the supplier's guidance. Confirm the make-up of magnesium soaps, sediments and foreign oil by laboratory analysis, and judge release agent changes together with the person responsible on the casting side.

With magnesium, safety comes first. Use protective equipment for coolants and additives as the product's safety data sheet, the SDS, directs, and limit skin contact with metalworking fluids and breathing in their mist (NIOSH, 1998). Magnesium sludge, wet chips and filter fleece give off hydrogen and can self-ignite, so do not collect them in sealed containers. Keep class D extinguishing agents for metal fires on hand, and never use water on a magnesium fire (DGUV, 2020). Plan large tank cleaning and sludge disposal with a specialist contractor or safety officer who knows the fire and explosion risks.

Sources

  1. Deutsche Gesetzliche Unfallversicherung [DGUV]. (2020). DGUV Information 209-090: Activities relating to magnesium. Retrieved November 2026. https://publikationen.dguv.de/widgets/pdf/download/article/3784
  2. International Organization for Standardization [ISO]. (1984a). ISO 6058:1984, Water quality — Determination of calcium content — EDTA titrimetric method.
  3. International Organization for Standardization [ISO]. (1984b). ISO 6059:1984, Water quality — Determination of the sum of calcium and magnesium — EDTA titrimetric method.
  4. Khan, T., Broderick, M., & Taylor, C. M. (2021). Investigating the industrial impact of hydraulic oil contamination on tool wear during machining and the development of a novel quantification methodology. The International Journal of Advanced Manufacturing Technology, 112(1–2), 589–600. https://doi.org/10.1007/s00170-020-06370-y
  5. National Fire Protection Association [NFPA]. (2022). NFPA 484: Standard for combustible metals.
  6. National Institute for Occupational Safety and Health [NIOSH]. (1998). Criteria for a recommended standard: Occupational exposure to metalworking fluids (DHHS (NIOSH) Publication No. 98-102). https://doi.org/10.26616/NIOSHPUB98102
  7. NürnbergMesse. (2020). Significance of release agents for die casting technology. EUROGUSS 365. Retrieved November 2026. https://www.euroguss.de/en/euroguss-365/2020/article/significance-of-release-agents-for-die-casting-technology
  8. Song, G. L., & Atrens, A. (1999). Corrosion mechanisms of magnesium alloys. Advanced Engineering Materials, 1(1), 11–33. https://doi.org/10.1002/(SICI)1527-2648(199909)1:1<11::AID-ADEM11>3.0.CO;2-N
  9. Spicer, A., Kosi, J., Billups, C., & Pajek, J. (1991). Machining magnesium with water base coolants (SAE Technical Paper 910415). SAE International. https://doi.org/10.4271/910415
  10. Tomac, N., Tønnessen, K., & Rasch, F. O. (1996). Safe machining of magnesium. In Advanced manufacturing systems and technology (CISM International Centre for Mechanical Sciences, pp. 177–184). Springer. https://doi.org/10.1007/978-3-7091-2678-3_19
  11. Zimmerman, J. B., Clarens, A. F., Hayes, K. F., & Skerlos, S. J. (2003). Design of hard water stable emulsifier systems for petroleum- and bio-based semi-synthetic metalworking fluids. Environmental Science & Technology, 37(23), 5278–5288. https://doi.org/10.1021/es034437t
  12. Zimmerman, J. B., Hayes, K. F., & Skerlos, S. J. (2004). Influence of ion accumulation on the emulsion stability and performance of semi-synthetic metalworking fluids. Environmental Science & Technology, 38(8), 2482–2490. https://doi.org/10.1021/es0340477

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.