Repainting is the usual response to paint peeling off a machine tool, but if whatever softened the film or lifted it from below is still there, the new paint tends to go the same way. What actually lies behind it can be amines and solvents attacking the film, high pH and concentration, paint with poor chemical resistance, spots that never dry, or cleaner that got into the coolant, and sometimes two or more at once.

Background

Inside the door of a machining centre, around the bed and on the chip conveyor cover, the paint swells, cracks and then falls away in flakes. The flakes ride the coolant, clogging filters and nozzles, and the bare steel underneath soon starts to rust. Beyond spoiling the machine's appearance, softened paint that dissolves and redeposits on parts or the machine can make cleaning harder or stop the machine working properly (Master Fluid Solutions, 2025).

A paint film is a thin layer of cured polymer on metal. No film keeps liquids out completely; water, oxygen and ions work their way into it over time (Sangaj & Malshe, 2004). A water-miscible coolant is water carrying many additives such as oil, emulsifiers, corrosion inhibitors and ingredients that hold the pH (Brinksmeier et al., 2015), so the film is exposed to far more than water. Paint therefore fails in one of three ways: ingredients in the fluid soften or dissolve the polymer, break it chemically, or get under the film and part it from the metal.

Machine tool design guidance likewise says the materials of machines that use coolant should be chosen with their compatibility with it in mind (VDI, 2024). One part of a machine stays sound while another peels because the fluid's ingredients, the type of paint and the time spent wet combine differently from spot to spot.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: photograph the peeling and sound areas, keep the flakes that fell off, note when it began and whether anything changed in the meantime in coolant, concentration, cleaning or paint, and compare that with the coolant's technical data sheet, the TDS, and the machine builder's paint specification.

Hypothesis 1: amines and solvents

If the paint trouble began after a change of coolant, especially to a synthetic or semi-synthetic fluid with less mineral oil and more water-soluble ingredients, look at the ingredients first. The same goes for when separately bought additives started going into the sump. Say a few weeks after switching to a new semi-synthetic, the paint inside the door and around the chip outlet has gone soft enough to push with a fingernail and leaves colour on gloves. On machines in the same plant still running the old coolant, the same spots are unchanged.

Synthetic and semi-synthetic coolants contain amines such as alkanolamines and ingredients such as glycols that mix with both water and oil (NIOSH, 1998). How far a liquid swells or dissolves a polymer can be judged by how close their solubility properties are; the closer they are, the more readily the liquid enters the polymer, swelling and softening it (Hansen, 2004). A coolant maker's technical bulletin likewise describes paint turning soft and sticky or going into solution as the sign of a solvent in the fluid dissolving the paint, or of paint that was not fully cured (Master Fluid Solutions, 2025). Amines are also bases and hold the fluid's pH high, which the next hypothesis takes up separately.

First set the amines, glycols and solvents in the present coolant beside those of the previous product, using the SDS and TDS. On the floor, rub sound paint a few times with a cloth soaked in the coolant and see whether colour comes off and whether a fingernail leaves a mark a little later. For a firmer answer, immerse panels coated with the same paint in coolant at working concentration and compare softening, blistering and discolouration with panels immersed in water. Immersion tests of how well a coating stands up to a liquid are set out in a standard (ISO, 2017).

If the coolant's ingredients appear to be softening the paint, there are two routes. One is to ask the coolant supplier for compatibility test data with that paint and, failing that, run panel immersion tests together and move to a product that is gentler on the film. The other, if the machine is to stay in service for years, is to switch at the next repaint to a paint that stands up to that coolant. Do not add separately bought additives without checking with the supplier.

Hypothesis 2: rich, high-pH fluid

On machines whose sump concentration creeps upward, a scene like this is possible: each time someone mentioned rust or short tool life, a little more concentrate went in, and evaporation was made up with strong premix instead of water. Measured, the concentration sits above the TDS range and the pH sits at the high end, and the paint has thinned and lost its gloss starting where the fluid splashes directly. Hot weather, when water evaporates quickly, tends to pile this up.

Water leaves the sump but the coolant ingredients stay, so unless top-ups are balanced with water the concentration rises easily (Byers, 2017). Higher concentration means more amine, solvent and alkali reaching the paint. Alkali can break a paint binder chemically. Binders with ester bonds, such as alkyds and polyesters, undergo saponification in alkali, the hydrolysis of those bonds, and turn soft and weak, which is why such paints are known for poor alkali resistance (Jones et al., 2017). The same fluid, then, attacks the film harder the richer it is and the higher its pH.

Concentration and pH show up as soon as they are measured. Read concentration with a refractometer, apply the supplier's correction factor and compare it with the TDS range, and measure pH with a pH meter. If there are records for the past few months, match when concentration began to climb with when the paint trouble appeared. Ask who tops up and how, and whether anyone pours in concentrate on the side. On the paint side, find the binder type in the paint specification and check whether it is an alkyd or polyester.

If the rich fluid proves to be the cause, start by bringing concentration back into the TDS range. Balance top-ups with premix at the set concentration or with water, and make topping up one person's job or an automatic mixer's so no one adds concentrate on the side. If rust or tool life was the reason concentration went up, look for the cause of that problem separately. Where the paint has an alkali-sensitive binder, assess the damage left once concentration is back in range and choose the paint for the repaint.

Hypothesis 3: weak paint system

If only certain areas peel under the same coolant at the same concentration, the paint itself is worth suspecting. Think of covers touched up on site with general-purpose paint during maintenance, areas painted without fully removing rust, and new or repaired machines filled with coolant and run straight after painting. On a machine where only the chip cover touched up at a service some years ago lifts off in large sheets while the factory paint right next to it is intact, the cause looks closer to the paint than to the fluid.

Paints fall into two broad groups: those that dry as their solvent evaporates, and those that cure by chemical reaction, such as two-part epoxies and catalysed polyurethanes. A coolant maker's technical bulletin explains that fluid seeps through the porosity left in a solvent-dried film and lifts small chips, while poor surface preparation or a porous primer lets fluid wick between paint and metal and lift large sheets; paint that is not fully cured stains or softens easily (Master Fluid Solutions, 2025). A crosslinked film, whose polymer chains are tied together in a network, resists solvents better than one with free chains, and the denser the network, the less it swells in a liquid (Jones et al., 2017).

The clues are in the flakes and what lies under them. Rust or oil on the back of a flake points to surface preparation; primer left on the metal with only the topcoat gone points to adhesion between coats. Cut a grid into sound and suspect areas with a knife, apply tape and pull it off, and compare adhesion by how much paint comes away; this cross-cut test is set out in a standard (ISO, 2020). Find the painting history and the TDS of the paint used to see whether it was solvent-drying or reaction-curing, and how long after painting the coolant went in.

If the cause is judged to be the paint, strip the damaged areas to bare metal, remove rust and oil, and repaint to the surface preparation and thickness the paint maker specifies. Choose a reaction-curing system suited to coolant-wetted areas with the paint maker, and decide only after immersion tests in the coolant actually in use. After painting, let it reach the full cure time the paint maker specifies before coolant touches it. When buying a new machine, asking about the paint specification and coolant compatibility as part of the purchase terms is another option.

Hypothesis 4: never-dry spots

If the peeling starts at particular spots and spreads, rather than across the whole machine, look at how long those spots stay wet. Typical ones are walls that coolant splashed from the nozzles runs down all the time, channels where fluid pools and never dries, and places where film tends to be thin, such as weld seams, bolt heads and edges. Picture a machine where a shallow pool always sits at one end of the channel under the table. Small blisters start there, breaking one releases fluid and rusty water, and the film lifts from the edges.

Where a spot is always wet, water and ions keep seeping into the film without a break (Sangaj & Malshe, 2004). If there is even a little soluble salt on the metal under the film, water is drawn towards it and a blister swells; osmotic blisters formed this way are a typical form of coating failure (Funke, 1981). Once water and oxygen reach the metal and corrosion begins, things speed up. Hydroxide ions formed under the film as oxygen is reduced turn that spot strongly alkaline, and the alkali breaks the bond between film and metal so the film lifts, which is called cathodic delamination (Leidheiser et al., 1983).

Checking means drawing a map. Mark the damaged areas on a drawing or photo of the machine and overlay nozzle directions, splash zones and places where fluid pools. If the damage coincides with wet areas and began at edges, seams or scratches, this hypothesis gains weight. Break one blister and see whether the metal beneath is rusted or sound. It also helps to note which spots are still wet hours after the machine stops.

Cutting the time spent wet is the first measure. Give pooling spots a way to drain, adjust nozzles and guards so fluid does not splash where it is not needed, and build up film on edges and seams with an extra coat as the paint maker recommends. Repair scratches and lifted spots while they are still small. For spots that stay wet whatever is done, consider a cover in a material that withstands the coolant instead of paint.

Hypothesis 5: cleaner in the sump

If the paint trouble started right after a coolant change or a thorough machine clean, the cleaner used then may have been left behind. It happens when a system cleaner was circulated and new fluid filled without rinsing, when the inside of the machine was wiped down with strong alkaline detergent or solvent, and when parts washer solution rides back to the machine tool on the parts. Take a plant that ran a system cleaner through the pipes during the year-end shutdown and refilled with new coolant straight away. After the first week of the new year, paint begins to lift on several machines at about the same time.

Cleaners are made to lift oil and dirt, and alkaline cleaners, solvents and emulsion cleaners are all used (MacKenzie, 2024). When these ingredients stay in the sump or reach the paint directly, alkali breaks the binder and solvent swells the polymer, as the two earlier hypotheses showed (Hansen, 2004; Jones et al., 2017). What the machine actually meets is then no longer the coolant originally chosen, so compatibility with the paint has to be judged against the fluid now in the sump.

In the maintenance records, line up the days system cleaners and cleaning chemicals were used, whether rinsing followed, and the day the paint trouble was first seen. Check the SDS of the cleaner used for alkali and solvent content. Comparing the pH and electrical conductivity of the sump fluid with freshly made fluid at the same concentration gives a sense of whether something got in. If parts return to the machine tool after the parts washer, see whether they arrive wet.

If cleaner is the cause, change how it is used. Use system cleaners only at the concentration and for the time their maker sets, rinse with water as instructed, then fill with new fluid. Choose detergents that do no harm to paint for cleaning the inside of the machine, and never wipe painted surfaces with strong solvents. If a lot has already got into the sump, change the fluid, and dry parts from the parts washer before sending them back to the machine tool.

Finding the cause

The five hypotheses need not be tested all at once. Start with what is easy to measure. Concentration and pH take minutes, and the dates of coolant changes, cleaning and touch-up painting are in the records. Panel immersion and adhesion tests take time, so they come next.

The shape and position of the damage are the first clue. Broad wetted surfaces turning evenly soft and sticky point to the fluid itself: its ingredients or a rich concentration. Paint lifting in large sheets, or only on touched-up areas, points to the paint and the surface preparation; blisters that start where fluid pools or splashes and then spread point to never-dry spots. If damage began on several machines at about the same time, look for what happened to all of them then, such as a coolant change or a major clean.

If that does not settle it, run a control trial. Immerse panels coated with the same paint, or pieces of cover taken from the machine, side by side in the current sump fluid, in fresh fluid made up at TDS concentration and in water. Damage only in the sump fluid points to rich concentration or cleaner that got in; damage in the fresh fluid too points to the match between coolant ingredients and paint. If all three panels stay sound while the machine still peels, time spent wet and surface preparation remain.

The final check is the film itself. Compare adhesion at damaged and sound areas with the cross-cut test, and examine the back of the flakes and the metal underneath. If needed, send flakes to the paint maker to confirm the binder type and how well it cured. After any change, photograph the same areas every few weeks to see whether the damage has stopped.

The hypotheses overlap easily. A rich fluid carries more amine and solvent, an alkali-sensitive paint gives way to that attack first, and a never-dry spot takes all of it for longest. In such cases first bring concentration and pH back into the TDS range and keep cleaners out, then turn to the paint and the wet spots, because repainting while the fluid is still unsettled gives no fair test of whether the new paint holds.

Limits and cautions

Suitable coolant concentration and pH ranges, paint surface preparation and thickness, and cure times differ by product, so numeric decisions follow the coolant TDS and the paint maker's guidance. If paint damage appears together with damage to other materials, such as way covers, seals or cable sheathing, tell the machine builder and review material compatibility together. For machines under warranty, consult the machine builder before repainting.

Safety matters too. For paint strippers, solvents and cleaners, follow the product's safety data sheet, the SDS, for protective equipment and ventilation, and avoid breathing dust from stripping paint. Metalworking fluids can harm health through skin contact and through breathing in mist (OSHA, n.d.), and the US National Institute for Occupational Safety and Health has set out a recommended exposure limit and control methods for reducing exposure to them (NIOSH, 1998). Clean or paint inside a machine only after it is fully stopped and locked out.

Sources

  1. Brinksmeier, E., Meyer, D., Huesmann-Cordes, A. G., & Herrmann, C. (2015). Metalworking fluids—Mechanisms and performance. CIRP Annals, 64(2), 605–628. https://doi.org/10.1016/j.cirp.2015.05.003
  2. Byers, J. P. (Ed.). (2017). Metalworking fluids (3rd ed.). CRC Press.
  3. Funke, W. (1981). Blistering of paint films and filiform corrosion. Progress in Organic Coatings, 9(1), 29–46. https://doi.org/10.1016/0033-0655(81)80014-3
  4. Hansen, C. M. (2004). 50 years with solubility parameters—Past and future. Progress in Organic Coatings, 51(1), 77–84. https://doi.org/10.1016/j.porgcoat.2004.05.004
  5. International Organization for Standardization [ISO]. (2017). ISO 2812-1:2017, Paints and varnishes — Determination of resistance to liquids — Part 1: Immersion in liquids other than water. https://www.iso.org/standard/71584.html
  6. International Organization for Standardization [ISO]. (2020). ISO 2409:2020, Paints and varnishes — Cross-cut test.
  7. Jones, F. N., Nichols, M. E., & Pappas, S. P. (2017). Organic coatings: Science and technology (4th ed.). Wiley.
  8. Leidheiser, H., Wang, W., & Igetoft, L. (1983). The mechanism for the cathodic delamination of organic coatings from a metal surface. Progress in Organic Coatings, 11(1), 19–40. https://doi.org/10.1016/0033-0655(83)80002-8
  9. MacKenzie, D. S. (2024). Cleaning for heat treatment – Part II. Thermal Processing. Retrieved November 2026. https://thermalprocessing.com/?p=29459
  10. Master Fluid Solutions. (2025). Machine tool compatibility – Paint (Technical Bulletin No. 030). Retrieved November 2026. https://masterfluids.com/na/en-us/technical-information/tb.php?tbid=030
  11. National Institute for Occupational Safety and Health [NIOSH]. (1998). Criteria for a recommended standard: Occupational exposure to metalworking fluids. DHHS (NIOSH) Publication No. 98-102. https://www.cdc.gov/niosh/docs/98-102/
  12. Occupational Safety and Health Administration [OSHA]. (n.d.). Metalworking fluids. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/metalworking-fluids
  13. Sangaj, N. S., & Malshe, V. C. (2004). Permeability of polymers in protective organic coatings. Progress in Organic Coatings, 50(1), 28–39. https://doi.org/10.1016/j.porgcoat.2003.09.015
  14. Verein Deutscher Ingenieure [VDI]. (2024). VDI 3035 Blatt 2, Material selection in the design of machine tools, manufacturing plants and peripheral equipment for the use of machining media. https://www.vdi.de/en/home/vdi-standards/details/vdi-3035-blatt-2-material-selection-in-the-design-of-machine-tools-manufacturing-plants-and-peripheral-equipment-for-the-use-of-machining-media-cooling-lubricants-forming-lubricants

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.