Spraying more often and more heavily is the usual response when open gear lubricant flies off, but if the reason it cannot stay on the teeth is left alone, only consumption rises and the teeth keep wearing. What actually lies behind it can be too little tack, faulty spraying, dust in the lubricant, a temperature out of the working range or poor mesh alignment, and sometimes two or more at once.

Background

Lumps of lubricant drop and pile up under the large girth gear that turns a kiln or a ball mill, and the inside of the gear guard and the floor around it are black and glossy. Yet the pinion teeth show patches of bright bare metal, with scratches running in the sliding direction. Plenty of lubricant seems to be going on, yet the teeth are meshing dry.

Lubricant thrown off is money lost, and it fouls floors and equipment, adding cleaning work and a slip hazard. Girth gears and pinions are large, costly parts, so replacing them means a long stop, and when a mill or kiln stops, the processes after it stop too. As worn teeth change shape, the mesh roughens and vibration and noise rise.

Unlike enclosed gears that run in oil inside a casing, open gears run under no more than a guard, and the lubricant is often sprayed on at intervals as a thin coat on the teeth (Errichello, 1997). The lubricant must therefore stay on the teeth until the next spray, while on a turning gear centrifugal force throws it outwards (DeWinter & Blok, 1974). If the film left in between cannot carry the mesh load, metal touches metal and the teeth wear. Industrial gear lubrication guidance, too, treats open gearing separately from enclosed drives (AGMA, 2016).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The first check never changes: compare the lubricant's technical data sheet, the TDS, and the spray system settings, meaning the spray interval and the amount per shot, with the gear maker's recommendations, and note the surface temperature of girth gear and pinion in service and the dust inside the guard.

Hypothesis 1: too little tack

This hypothesis is the first suspect after a switch to a cheaper or easier-to-source lubricant, or when an enclosed gear oil or a general-purpose grease stands in on an open gear. Lubricant that separated in long storage and went on unmixed belongs here too. Take the month when purchasing swapped the open gear lubricant for another product to cut the unit price. The spray settings are unchanged, but more lubricant than before drops into the tray under the pinion, and thin trails run down the side of the girth gear.

One property an open gear lubricant needs is tack, the tendency to cling to metal and stretch into strings rather than let go. It usually comes from a small addition of high-molecular-weight polymer, and such tackifiers are used to reduce dripping and fling-off (Litt, 2003). Without enough tack, the lubricant cannot hold against centrifugal force and the squeeze of the mesh and leaves the teeth, so the film left until the next spray is too thin. Where water is sprayed or rain gets in, the ability to cling matters even more, and there is a standard test of how well a grease stays on a metal surface under a water spray (ASTM International, 2020).

Tack can be compared roughly by hand. Put the new and the current lubricant between two fingers at the same temperature, spread them and compare how far each strings out, then check whether the film left on the teeth in service is even and whether bare metal appears just before the next spray. Collecting what falls into the tray over a set period and weighing it gives a figure for how much of the sprayed amount is thrown off.

The fix starts with the choice of lubricant. Go back to the dedicated open gear lubricant the gear maker recommends, or choose a product whose TDS meets that standard. When changing products, scrape off the old lubricant and inspect the teeth often until the new film is evenly established. Lubricant that has separated in storage is either remixed as the supplier instructs or not used.

Hypothesis 2: faulty spraying

This hypothesis is worth checking after the interval or the amount per shot on an automatic spray system has changed, when nozzles clog or are knocked out of line, or when the atomising air pressure drops. If the spray interval was stretched to meet an order to cut lubricant consumption, suspect that change first. A fitter took off the mill pinion's spray nozzles, cleaned them and refitted them. Since then one end of the girth gear face is glossy while the other looks dry, and the teeth on the dry side are turning brighter first.

An open gear does not receive lubricant on every turn; it runs on a thin film sprayed at set intervals (Errichello, 1997). Each sprayed film has to last until the next shot, so if the interval is too long or each shot too small, the film wears and flies off in between, leaving spells when the teeth mesh dry. Spraying too much at once does not build a correspondingly thicker film either, since the surplus squeezed out of the mesh is flung off by the turning gear (DeWinter & Blok, 1974). A clogged or tilted nozzle wets only part of the face width rather than all of it, leaving dry patches on the same tooth.

Looking at the spray system directly is quickest. Trigger it once by hand to see whether each nozzle's pattern covers the full face width and whether any is blocked, then spray a set number of shots, measure the output and check it against the setting. After that, compare the teeth just after a spray with the teeth just before the next one, looking for places where bare metal shows before the next shot. Check the air pressure and the lubricant tank low-level alarm records as well.

When the spray turns out to be the cause, return the interval and amount to the range the gear maker and lubricant supplier recommend, and add nozzle cleaning and spray pattern checks to routine inspection. To cut consumption, look first at spreading the pattern evenly across the face width rather than stretching the interval. Straight after a change of lubricant or gear, also check whether the maker sets separate initial spray conditions.

Hypothesis 3: dust in the lubricant

This hypothesis moves to the front for open gears in dusty plants such as cement works, mines and steelworks, when guard seals are damaged or the gear runs with the guard open. Cleaning with compressed air nearby or dust blowing off a neighbouring conveyor does the same. Take the girth gear on a cement kiln. The rubber seal at the bottom of the guard has been torn for some weeks, and the lubricant on the teeth has turned from glossy black to something like grey paste.

A lubricant that clings well to the teeth also holds on to settling dust. Hard particles caught in it are dragged between the meshing teeth and cut the surfaces like an abrasive; in tests of this wear by particles trapped between two surfaces, more angular particles caused more wear, and particle toughness and embedding in the surface also changed the result (Stachowiak & Stachowiak, 2001). The effect of lubricant contamination on gear wear has also been studied in gear tests (Sari et al., 2007). In sliding contact tests, solid particles in the lubricant made film thickness fluctuate markedly and raised friction, and wear sped up with sand particles present and as temperature rose (Sari et al., 2010).

Scrape a little lubricant off the teeth and rub it between the fingers to feel for grit, then dissolve the same sample in solvent and filter it to see the amount and shape of the particles left. A laboratory can look at elements from dust, such as silicon, alongside wear elements such as iron. Walk round the guard seals, inspection doors and drains to find where dust gets in, and note how much has built up inside the guard.

With dust, closing off its way in comes first. Repair the guard seals and inspection doors, stop compressed-air cleaning nearby, and if needed discuss keeping the inside of the guard at slightly raised pressure with the equipment maker. Scrape the grit-laden lubricant off the teeth and out of the tray and build a fresh film with new lubricant. Photograph scratches already on the teeth and check at the next inspection whether they have spread.

Hypothesis 4: wrong temperature

Trouble comes where temperature leaves the lubricant's working range. A winter-morning restart or an open gear standing outdoors is one extreme, and a girth gear taking radiant heat close to a kiln shell is the other. Sometimes the gear itself runs hot enough to leave the range. Here is an outdoor drive gear on a midwinter Monday morning after a weekend shutdown. The lubricant leaves the nozzle in heavy drops instead of a fine mist, and the teeth show lumpy patches mixed with bare gaps.

A lubricant's viscosity changes strongly with temperature, stiffening in the cold and thinning in the heat (Stachowiak & Batchelor, 2014). Too cold, and the spray system cannot spread the lubricant evenly and it will not spread thinly on the teeth, leaving gaps in the mesh. Too hot, and the lubricant thins, runs off and is flung away easily, and the film that remains is thinner. That is why industrial gear lubrication guidance has ambient temperature and application method weighed together when an open gear lubricant is chosen (AGMA, 2016).

Temperature shows as soon as it is measured. Use an infrared thermometer on the girth gear and pinion teeth in service, and measure the spray unit, lubricant tank and lines too. Compare the readings with the working range and minimum spray temperature in the TDS, and search the records for whether the symptoms cluster when temperature shifts, at a change of season or just after start-up.

If temperature is out of range, agree with the supplier on a grade suited to it, or on separate grades by season. In cold locations, consider insulating or heating the tank and lines; in hot ones, add a shield against radiant heat. Look for the reason a gear itself runs hot on the mesh side as well. After a grade change, recheck and record the spray pattern and tooth film on the coldest morning and the hottest day of the year.

Hypothesis 5: poor mesh alignment

The mesh can go out of line after a foundation settles, a kiln shell grows with heat, or pinion bearings are replaced and the pinion reset. A loose girth gear mounting that lets the gear wobble throws the mesh out too. On a ball mill restarted after a pinion bearing change, only one end of the pinion face is unusually bright, and the lubricant there disappears quickly. At the other end of the same teeth, the lubricant sits thick.

When the mesh is true, load spreads evenly across the face width, but even a slight misalignment of the two shafts changes where the teeth touch and how the load is shared (Li, 2015). With load concentrated at one end, pressure and friction heat rise there, the lubricant is squeezed out and thinned, and wear starts where the film is thinnest. The lubricant then goes unused at the other end and runs short where contact is heaviest. Alignment therefore cannot be separated from lubrication, and the mill and kiln gearing standard covers installation, alignment, maintenance and lubrication together in its annexes (AGMA, 2015).

The contact pattern is the clearest evidence. Coat the teeth thinly with marking compound, turn the gear slowly, and where and how much the marks cover across the face width and up the tooth height show the state of alignment. Methods for checking contact patterns are set out in gear inspection recommendations (ISO, 1998). In service, use an infrared thermometer on both ends of the pinion face to see whether one end runs noticeably hotter. Recording tooth wear and pitting with photographs, in the terms of the gear damage nomenclature standards, lets you speak the same language as suppliers and specialists (AGMA, 2014; ISO, 2022).

If alignment is the cause, lubricant will not fix it. Reset the pinion with the gear maker or an alignment specialist, and on equipment such as kilns that changes shape with heat in service, check again once it has reached running temperature. Inspect the foundation bolts and girth gear mounting for looseness too, and after realignment, repeat the contact pattern and end-temperature checks the same way and keep the records.

Finding the cause

The spray system and temperature can be checked without stopping, so rule them out first. Look at the nozzle patterns, the amount per shot and the tooth temperatures, and inspect the dust inside the guard on the same day. The lubricant product and alignment come next, since trying another lubricant takes time and checking alignment means a stop.

The shape and place of the wear point to the cause. Wear and polish concentrated at one end of the face point to mesh alignment, and dry marks on only part of the face to a blocked nozzle or a misaimed spray. Scratches spread evenly over the whole tooth with greyed lubricant point to dust, and if far more lubricant is falling into the tray while the film on the teeth stays even, look at tack or temperature first.

Timing matters too. After a change of lubricant, suspect tack first; after new spray settings or nozzle work, the spray; when problems cluster at a change of season or a restart, temperature; and after a bearing change or foundation work, alignment. If the same spot keeps wearing even after the lubricant has been changed, lean towards alignment.

If two or more remain, change one thing at a time. With the spray interval and amount back in the recommended range, record the lubricant falling off and the state of the teeth over a set period, and only if nothing changes move on to the next variable. Always compare on the same yardsticks: the same running hours, photographs of the same teeth, the weight of lubricant collected in the tray.

The hypotheses overlap easily. Misalignment heats one end, where the lubricant thins and flies off, and dust caught where the film has thinned speeds up wear further. Lubricant stiffened on a cold day disturbs the spray pattern as well. In such cases, put the mechanical conditions such as alignment and spray right first, then revisit the choice of lubricant. While the mechanical side is unsettled, the effect of a lubricant change cannot be judged fairly.

Limits and cautions

The right lubricant type, spray interval and amount, working temperature range and alignment tolerances differ with gear size, speed, load and equipment, so numeric decisions follow the gear maker's instructions and the lubricant TDS. Crack inspection, realignment and re-machining of large girth gears are specialist work. If a tooth has broken or a crack is suspected, do not keep running on floor judgement alone.

Open gears carry a high risk of hands or tools being drawn into the mesh. Any work that puts a hand inside the guard, such as nozzle checks, contact pattern checks or cleaning the teeth, is done only with the equipment stopped and locked out, following the rules for controlling hazardous energy (OSHA, n.d.). Take temperatures in service only through inspection doors or at designated measuring points. Handle lubricants and cleaning solvents with the protective equipment and ventilation set out in the safety data sheet, the SDS, and clean up lubricant on the floor straight away so no one slips.

Sources

  1. American Gear Manufacturers Association [AGMA]. (2014). ANSI/AGMA 1010-F14, Appearance of gear teeth — Terminology of wear and failure.
  2. American Gear Manufacturers Association [AGMA]. (2015). ANSI/AGMA 6014-B15, Gear power rating for cylindrical shell and trunnion supported equipment. https://webstore.ansi.org/standards/agma/ansiagma6014b15
  3. American Gear Manufacturers Association [AGMA]. (2016). ANSI/AGMA 9005-F16, Industrial gear lubrication. https://webstore.ansi.org/standards/agma/ansiagma9005f16
  4. ASTM International. (2020). ASTM D4049-20, Standard test method for determining the resistance of lubricating grease to water spray. https://store.astm.org/d4049-20.html
  5. DeWinter, A., & Blok, H. (1974). Fling-off cooling of gear teeth. Journal of Engineering for Industry, 96(1), 60–70. https://doi.org/10.1115/1.3438331
  6. Errichello, R. (1997). Gear lubricant selection and application. In E. R. Booser (Ed.), Tribology data handbook. CRC Press. https://doi.org/10.1201/9781420050479.ch67
  7. International Organization for Standardization [ISO]. (1998). ISO/TR 10064-4:1998, Cylindrical gears — Code of inspection practice — Part 4: Recommendations relative to surface texture and tooth contact pattern checking.
  8. International Organization for Standardization [ISO]. (2022). ISO 10825-1:2022, Gears — Wear and damage to gear teeth — Part 1: Nomenclature and characteristics. https://www.iso.org/standard/78719.html
  9. Li, S. (2015). Effects of misalignment error, tooth modifications and transmitted torque on tooth engagements of a pair of spur gears. Mechanism and Machine Theory, 83, 125–136. https://doi.org/10.1016/j.mechmachtheory.2014.09.011
  10. Litt, F. (2003). Tackiness and antimisting additives. In L. R. Rudnick (Ed.), Lubricant additives: Chemistry and applications (pp. 355–361). Marcel Dekker. https://doi.org/10.1201/9780824747404.ch12
  11. Occupational Safety and Health Administration [OSHA]. (n.d.). Control of hazardous energy (lockout/tagout). U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/control-hazardous-energy
  12. Sari, M. R., Haiahem, A., & Flamand, L. (2007). Effect of lubricant contamination on gear wear. Tribology Letters, 27(1), 119–126. https://doi.org/10.1007/s11249-007-9215-z
  13. Sari, M. R., Ville, F., Haiahem, A., & Flamand, L. (2010). Effect of lubricant contamination on friction and wear in an EHL sliding contact. Mechanika, 82(2), 43–49. https://doi.org/10.5755/j02.mech.15517
  14. Stachowiak, G. B., & Stachowiak, G. W. (2001). The effects of particle characteristics on three-body abrasive wear. Wear, 249(3–4), 201–207. https://doi.org/10.1016/S0043-1648(01)00557-9
  15. Stachowiak, G. W., & Batchelor, A. W. (2014). Engineering tribology (4th ed.). Butterworth-Heinemann.

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.