KALTECKOREA

BlogApplication notes

Why does the paint film look like orange peel?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Coatings & Surface Treatments

Adding more thinner is the usual response to orange peel, but the texture is set by how far the bumps in the sprayed film flow out before it sets, so changing thinness alone tends to bring it back and can invite other defects such as sags. What actually lies behind it can be high viscosity, thinner that evaporates too fast, the wrong spray pressure or distance, film build off target, or a temperature too low or too high, and sometimes two or more at once.

Background

Look at a finished panel at a low angle under the lights and the surface shows a fine, bumpy texture like orange peel, with the reflected fluorescent tubes rippling as if seen through water. Protection may look unaffected for now, but where appearance is a quality criterion, that panel needs sanding and polishing or a repaint. That costs extra paint, labour and line time, and when the same texture is back the next day, deliveries slip. Heavily textured panels sometimes go out as they are and come back from the customer's inspection.

Sprayed paint arrives as small droplets that pile up, so the film starts out with an uneven surface. Surface tension pulls those bumps flat while viscosity resists the flow; the bumps decay at a rate proportional to surface tension and to the cube of film thickness, and inversely proportional to viscosity and to the fourth power of the spacing of the texture (Orchard, 1963). One study that filmed spraying at high speed concluded that orange peel is not produced by evaporative convection in the wet film but is unevenness formed during spraying that has not flowed out by the time the film sets (Tachi et al., 1985). Another study, by contrast, observed that in very thick films, surface tension flows driven by differences in solvent concentration persisted until drying and left orange peel behind (Saranjam et al., 2016).

So orange peel is the outcome of two things: how large the initial bumps were, and how far they flowed out before the film set. Spray pressure and distance set the initial bumps; viscosity, thinner and temperature set the time available to flow and the resistance to it; film thickness sets how fast it flattens. A study comparing simulated and measured paint film levelling likewise showed the initial film shape and the viscosity governing levelling (Seeler et al., 2017). In a study that measured both evaporation rate and flow behaviour, the factor that governed levelling most was the build-up of viscosity as the film dried (Wang et al., 2019).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: keep a textured panel and a good one side by side, record that day's paint flow time and temperature, thinning ratio and thinner type, gun settings and wet film thickness, and compare them with the paint's technical data sheet, the TDS.

Hypothesis 1: viscosity too high

Viscosity is the first suspect when thinning was short of the set amount or done by eye, when solvent has evaporated from paint left with the lid off, or when a higher-solids paint was introduced and the old thinning ratio kept. Paint that has stood a long time in a circulation line or pressure pot belongs here as well. Take a line that runs all day from one generous batch mixed in the morning. Panels painted just after the tin was opened are smooth, but the texture coarsens through the afternoon and the gun now and then spits a heavy drop. Switch to a freshly mixed batch and the finish is smooth again.

Viscosity is the resistance to flow. Paint that is too viscous gives orange peel and gun spatter and fails to knit together, while paint that is too thin gives runs and sags (USACE, 1995). Thick paint is at a disadvantage from atomisation onwards. Droplet size depends on fluid properties as well as on flow rate and atomiser conditions, and it moves together with the wavelengths measured on the finished appearance (Ellwood et al., 2014). Once on the surface, the higher the viscosity the more slowly the bumps flatten, and lowering film viscosity reduced orange peel (Tachi et al., 1985).

Viscosity can be measured on the spot with a flow cup. The cup, with an orifice of set diameter, is filled with paint and the time for it to drain is measured; because the result depends on temperature, the standard includes an informative conversion of flow times between temperatures (ISO, 2019a). Take paint headed for the gun just before application and compare it with the TDS flow time using the same cup and the same temperature basis, and log values just after mixing and a few hours later side by side. If flow time lengthens over the day and the texture coarsens with it, the cause lies with viscosity.

When viscosity reads high, add the specified thinner within the TDS range, measured by scale or graduated cup, then recheck flow time. Thinning beyond the range gives thin films and sags, so respect the upper limit too. Mix only what will be used in one go, and keep tins and tanks closed. After a change to a product with different solids, reset the thinning ratio from the new TDS, and have the line operator measure and log flow time at the start and middle of every shift.

Hypothesis 2: thinner too fast

This hypothesis comes up when the specified thinner ran out and a general-purpose one was used, when a fast thinner from winter stayed in use after the weather warmed, or when stronger booth airflow sweeps quickly across the painted surface. Work that lays many overlapping passes over a large area is especially exposed. In a week when thinner stock ran out, a thinner from a different source was brought in and flow time was set exactly as usual. Yet the surface came out rough with lower gloss, and the texture stands out most in the bands where passes overlap.

A solvent has two jobs: keep the paint fluid while it is applied, then leave the film. It must evaporate fast enough to prevent runs and sags, but a solvent that is too volatile causes solvent pops, loss of gloss, dry spray, and poor wetting and flow, which is why paints use a blend of fast and slow solvents (USACE, 1995). With a faster thinner, droplets are already thickening in flight, and once on the surface their viscosity climbs quickly, cutting the time the bumps have to flatten. A study that built a levelling model including both evaporation and the change in viscosity likewise named viscosity build-up as the dominant factor in levelling (Wang et al., 2019).

Evaporation is not even across the surface either. In solvent-borne paints, solvent depletes first where the film is thinner, which changes the surface tension there, and the flow driven by these surface tension differences decides the course of levelling (Overdiep, 1986). A three-dimensional simulation of a film of resin and volatile solvent likewise showed surface tension gradients created by evaporation changing the levelling process (Eres et al., 1999). The faster the evaporation, the more likely the film sets before such differences even out, leaving them in place.

Start with the label on the thinner can. Check whether the thinner in use is the one the TDS specifies, whether its speed suits the season, and when it changed, against the date the rejects rose. Then thin the same paint with each of the two thinners to the same flow time, spray test panels at the same settings, and compare the surfaces and the time until they are no longer tacky to the touch. Measure booth air speed and flow direction as well, and compare them with normal values.

If the thinner is the cause, return to the thinner the TDS specifies, and in hot weather switch to the slower thinner or retarder the supplier recommends. A thinner that is too slow invites sags in turn, so choose its speed for the season and the booth conditions together with the supplier. Adjust booth air speed and direction so strong air does not sweep over freshly painted surfaces, and whenever the thinner changes, prove it on test panels before it goes on the line.

Hypothesis 3: pressure or distance

Suspect the spray conditions when the texture increased after a change of gun or nozzle, a change of painter, or a rise in fluid pressure alone to keep up output. The same applies when an undersized compressor or a longer hose lets air pressure at the gun drop, or when reaching high or deep areas puts the gun far from the surface or at an angle. Picture a day when fluid pressure at the pressure pot went up a step to raise output, while the atomising air was left as it was. The texture coarsens across the whole panel, and the upper corners that are hard to reach come out gritty, as if sand had been sprinkled on.

In an air-atomising gun, compressed air jetting from the nozzle breaks the paint stream into fine droplets and carries them to the surface. Excessive fluid pressure sends the paint out faster than the air jets can properly atomise, so pressure is kept as low as possible to prevent overspray and flooding yet high enough to support atomisation (USACE, 1995). Coarse droplets make larger initial bumps, and finer atomisation lowered the height of those initial bumps and reduced orange peel (Tachi et al., 1985). With rotary atomisers too, the conditions that set droplet size moved together with the wavelengths of the finished appearance (Ellwood et al., 2014).

Distance sets how long droplets are in flight. Too far, and droplets lose solvent on the way and land nearly dry as dry spray; too close, and paint piles up at once into runs and sags. The same manual puts the gun-to-surface distance at about 200 to 250 mm for conventional air spray and about 300 to 460 mm for airless, with the gun held perpendicular to the surface and each pass overlapping the previous one by 50% (USACE, 1995). Dry droplets cannot flow any further on the film, so areas sprayed from too far go past coarse texture to a gritty finish.

Fit a gauge at the gun inlet to read actual air pressure while spraying, and compare fluid pressure and nozzle size with the TDS and the gun maker's recommendations. Give a short burst onto a scrap panel or paper with the gun held still to see whether the pattern shape and droplet size are even. Watch the painter at work and measure gun distance, angle, travel speed and overlap, and compare whether the worst texture coincides with hard-to-reach areas.

Start the settings again from the TDS and the gun maker's recommendations. If more output is needed, do not raise fluid pressure alone; match nozzle size or atomising air with it, and if air is short, deal with compressor capacity and hose length. Provide staging or extension guns so distance and angle can be held in high or deep areas, and align individual painters' habits on test panels.

Hypothesis 4: film build off target

Look at this hypothesis when gun travel sped up along with the line, when a colour with good hiding tempts painters to finish in one thin coat, and at edges and pass ends where the film tends to run thin. Laying it on thick in one go to save passes belongs here as well. On panels after a line speed increase, the centre is reasonably smooth but the texture sharpens towards the ends of passes and the panel edges. A wet film gauge there reads lower than at the centre.

Thickness matters because the levelling rate is proportional to the cube of film thickness (Orchard, 1963). Halve the film and the same bumps flatten at one eighth of the speed, so thin areas barely level before they set. In actual sprayed films, too, thicker films had less orange peel (Tachi et al., 1985). That does not make thicker always better. In very thick films, cellular flows driven by differences in solvent concentration continued until drying and left a wavy structure on the surface, while in thin films the same patterns disappeared within minutes (Saranjam et al., 2016). Thick films also raise the risk of runs and sags.

The quickest way to check thickness is a wet film gauge just after application. A comb gauge is pressed square to the surface and read between the last tooth wetted and the first one dry, and standard methods are set for this as well as for dry film thickness (ISO, 2019b). Measure the centre, edges, pass ends and corners of the panel, and map whether the worst texture coincides with the lowest readings. If texture appears only where the film is very thick, look at excess build; if it gathers in thin areas, look at shortfall.

Bringing thickness within the wet and dry film ranges in the TDS is the remedy. If the film is short, slow the gun and keep to the overlap, and for paints that cannot reach the range in one coat, apply two coats with the specified wait between them. If over-thinning has lowered the solids, correct the thinning first. If the film is excessive, reduce output or the number of passes, and issue wet film gauges so painters can check as they go.

Hypothesis 5: too cold or too hot

This hypothesis comes forward when temperatures differ from normal: at the turn of the seasons, in booths without heating or cooling, with paint or parts brought in from an outdoor store, or with steel heated by the sun. All the more so when the same paint at the same settings gives different texture depending on time of day or weather. One example is steel plate brought in from an outdoor yard on a summer afternoon after sitting in the sun, and painted straight away without cooling. Panels painted in the morning were smooth, but these come out with less gloss, a rougher surface and gritty patches here and there.

Temperature moves viscosity and evaporation together. Paint stored somewhere cold becomes very viscous, and thinning it excessively to make it sprayable reduces solids and gives a thinner dry film. In the shop, hot spray heats paint to 66 to 71 °C to lower viscosity without extra thinner, which also allows atomising at lower pressure with less overspray, but catalysed paints such as two-part products cannot be used because they would set up in the equipment (USACE, 1995). The same dependence is why the flow-cup standard carries a separate conversion between temperatures (ISO, 2019a).

High temperature does harm another way. Above 32 °C, pot life can shorten or solvents flash off too rapidly, giving incomplete film formation, poor wetting, dry spray and loss of gloss (USACE, 1995). Since the rise in viscosity with evaporation is what governs levelling most, the bumps have that much less time to flatten on a hot surface (Wang et al., 2019). On a cold surface, by contrast, the paint stays thick and flows sluggishly.

Three thermometers will do. Measure the temperature of the paint headed for the gun, the surface temperature of the parts to be painted and the air temperature in the booth, and compare them with the application conditions in the TDS. Re-measure flow time at the temperature on the spot, and sort reject records by time of day, weather and where the parts came from to see whether the texture clusters in particular temperature conditions. Spraying one test panel early in the morning and one at midday at the same settings shows the difference at once.

Bring paint and parts to the temperature of the painting area in advance. Store paint near the painting area from the day before, and leave parts that were exposed to sun or cold until they approach room temperature before painting. If heating or cooling the booth is not practical, agree thinner speeds for each season with the supplier, and avoid painting at times when temperature falls outside the TDS range. On a shop line with non-catalysed paint, heated spray to set viscosity without thinning is another option to review.

Finding the cause

Five hypotheses do not mean five separate investigations. Rule them out one at a time, starting with what is easy to measure. Paint temperature and flow time, thinning ratio and thinner type, and gun pressure can be checked in a few minutes without stopping the line, and wet film thickness is read as soon as the paint is on. Things tied to working habits, such as distance and angle, are observed after that.

The first clues are where and when the texture appears. If it is even across the panel and improves with freshly mixed paint, suspect viscosity; if it varies with time of day or season, suspect temperature and thinner speed. If it gathers at pass ends, edges and hard-to-reach areas, look at distance, angle and film thickness. If the surface goes beyond orange peel to a gritty, matt finish, droplets dried in flight as dry spray, so check for excessive distance, a thinner that is too fast and a hot surface first.

Judging by eye alone varies with the person and the lighting, so turn it into numbers. A test method that rates the sharpness of reflected images from 0 to 100 correlates well with visual ratings, but the value by itself does not say what caused the loss of sharpness (ASTM International, 2023). Whether the paint itself flows well can be gauged in the laboratory with a draw-down levelling test, which looks at how far ridges drawn with a bar disappear, though that standard is written for architectural paints (ASTM International, 2024). If the paint levels well in the laboratory but textures only on the line, the evidence leans towards spray conditions, thickness and site temperature.

If that still does not settle it, run control trials on test panels. Spray one panel at the reference settings, then change thinner type, atomising air pressure, gun distance, film thickness or paint temperature one at a time, one panel each, and compare them under the same lighting with the same measurement. Change only one thing at a time, or there is no telling which one worked. After the fix, count reworked panels over a set period on the same basis as before, and the job is done only when that figure is back to its earlier level.

The hypotheses can overlap. On a cold day, heavily thinning paint that has thickened brings viscosity into line but thins the film, and raising fluid pressure to force thick paint through the gun coarsens atomisation. On a hot day, a hot part combined with a fast thinner goes all the way to dry spray. In such cases, set paint and part temperature first, then viscosity at that temperature, and only then gun settings and film thickness. Gun settings depend on viscosity, so while viscosity is unsettled, no amount of adjusting the gun will give a steady result.

Limits and cautions

Suitable flow time, thinning ratio, thinner type, gun pressure and distance, wet and dry film thickness and application temperature differ by paint and equipment, so numeric decisions follow the product's TDS and the gun maker's guidance. Set the pass mark for appearance by the standard and measurement method agreed with the customer, and judge whether sanding and polishing can fix a panel from the film thickness that would remain. For coatings that must protect, do not let a cosmetic fix take the film below its specified thickness.

Safety matters too. Solvent-borne paints and thinners ignite easily, so spraying flammable materials follows the rules on booths, ventilation and ignition sources (OSHA, n.d.). For paints and thinners, follow the product's safety data sheet, the SDS, for protective equipment and respiratory protection, and run heated spray equipment at the temperatures its maker specifies. Release pressure before inspecting the gun or cleaning the nozzle, and never point the gun at anyone.

Sources

  1. ASTM International. (2023). ASTM D5767-18(2023), Standard test method for instrumental measurement of distinctness-of-image (DOI) gloss of coated surfaces. https://store.astm.org/d5767-18r23.html
  2. ASTM International. (2024). ASTM D4062-24, Standard test method for leveling of paints by draw-down method. https://store.astm.org/d4062-24.html
  3. Ellwood, K. R. J., Tardiff, J. L., & Alaie, S. M. (2014). A simplified analysis method for correlating rotary atomizer performance on droplet size and coating appearance. Journal of Coatings Technology and Research, 11(3), 303–309. https://doi.org/10.1007/s11998-013-9535-x
  4. Eres, M. H., Weidner, D. E., & Schwartz, L. W. (1999). Three-dimensional direct numerical simulation of surface-tension-gradient effects on the leveling of an evaporating multicomponent fluid. Langmuir, 15(5), 1859–1871. https://doi.org/10.1021/la980414u
  5. International Organization for Standardization [ISO]. (2019a). ISO 2431:2019, Paints and varnishes — Determination of flow time by use of flow cups. https://www.iso.org/standard/73851.html
  6. International Organization for Standardization [ISO]. (2019b). ISO 2808:2019, Paints and varnishes — Determination of film thickness. https://www.iso.org/standard/71583.html
  7. Occupational Safety and Health Administration [OSHA]. (n.d.). 1910.107, Spray finishing using flammable and combustible materials. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/laws-regs/regulations/standardnumber/1910/1910.107
  8. Orchard, S. E. (1963). On surface levelling in viscous liquids and gels. Applied Scientific Research, Section A, 11(4–6), 451–464. https://doi.org/10.1007/BF03184629
  9. Overdiep, W. S. (1986). The levelling of paints. Progress in Organic Coatings, 14(2), 159–175. https://doi.org/10.1016/0033-0655(86)80010-3
  10. Saranjam, N., Chandra, S., Mostaghimi, J., Fan, H., & Simmer, J. (2016). Orange peel formation due to surface tension-driven flows within drying paint films. Journal of Coatings Technology and Research, 13(3), 413–426. https://doi.org/10.1007/s11998-015-9752-6
  11. Seeler, F., Hager, C., Tiedje, O., & Schneider, M. (2017). Simulations and experimental investigation of paint film leveling. Journal of Coatings Technology and Research, 14(4), 767–781. https://doi.org/10.1007/s11998-017-9934-5
  12. Tachi, K., Okuda, C., & Suzuki, S. (1985). Mechanism of orange peel defect formation in sprayed coatings. Journal of the Japan Society of Colour Material, 58(5), 257–263. https://doi.org/10.4011/shikizai1937.58.257
  13. U.S. Army Corps of Engineers [USACE]. (1995). Painting: New construction and maintenance (EM 1110-2-3400). Department of the Army.
  14. Wang, X., Huang, Y., Weinell, C. E., Olsen, S. M., & Kiil, S. (2019). Leveling kinetics of coatings with solvent evaporation and non-Newtonian rheology. Progress in Organic Coatings, 132, 169–177. https://doi.org/10.1016/j.porgcoat.2019.03.033

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.