KALTECKOREA

BlogApplication notes

Why does stainless steel rust after passivation?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Corrosion Prevention

Passivating again under the same conditions is the usual response when passivated stainless steel rusts, but if the cause lies before or after the treatment, in the grade or in the service environment, the rust comes back. What actually lies behind it can be leftover free iron, wrong acid conditions, a treatment that does not suit the grade, poor rinsing, chloride exposure or heat tint left on the welds, and sometimes two or more at once.

Background

A batch of stainless steel parts goes out passivated and certified, and days or weeks later word comes back of brown rust spots or rust streaks. The customer believed stainless steel does not rust, so the whole treatment is called into question and the shipment has to be recalled and reprocessed. Where the surface is the product, as in food, medical or semiconductor equipment, one rust spot is grounds for rejection, and if the rust grows into pitting, corrosion that bores in like a pinhole, it shortens the part's life as well.

Stainless steel resists rust because its surface carries a very thin chromium-rich oxide film, the passive film. It is only 1 to 3 nm thick, yet it stops the metal from dissolving (Olsson & Landolt, 2003). Passivation is not a coating that lays this film on. The standard defines it as removing exogenous iron or iron compounds from the surface by dissolving them in acid without significantly attacking the steel itself (ASTM International, 2017a). It clears the way for the film to re-form evenly on a clean surface.

So rust after passivation follows one of three paths. The treatment did not clear all the contamination and weak spots from the surface, the treatment itself did not suit the grade, or the environment after treatment went beyond what that grade's passive film can bear. Where and when the rust appeared is the clue that separates the three.

In such cases the technical team sets up the six hypotheses below and rules them out one by one. The start is always the same: pull the grade certificate of the rusted parts and the lot's passivation record, meaning acid type, concentration, temperature, time, rinsing and drying, compare them with the specification applied, and note whether the rust appeared right after treatment or in service, and where on the part it sits.

Hypothesis 1: leftover free iron

This hypothesis comes up first in shops that machine and move stainless steel with the same tools, fixtures and tongs used for carbon steel parts, that share grinding wheels or wire brushes with carbon steel, or that assemble stainless steel next to carbon steel machining. The same goes for parts touched up again after passivation or set down on carbon steel supports. Take a lot of stainless sleeves machined on a lathe that had just been turning carbon steel shafts. About a week after passivation and shipment, small rust spots appeared in rows along the machining marks, and rust also showed where the chuck had gripped.

Iron picked up in machining and handling is embedded in the surface as particles of tool steel or carbon steel, and it is exactly what passivation is meant to remove. In experiments where iron was deliberately smeared onto stainless steel, the iron dragged the surface potential down to the level of iron, removed the stainless steel's ability to passivate on its own, and rusted at once in salt fog, staining the surface. Passivating to remove the iron made all of this disappear (Enos & Wichhart, 2021). If the iron is not fully dissolved, or new iron arrives after treatment, the particles rust in damp air into brown spots, and the stainless steel beneath them is left without an even film.

The pattern of the spots is the first clue. Spots lined up along machining marks, where tools or chucks touched, or on faces that rested on supports point to iron contamination. The tests are set out in the standards. The passivation specification finds remaining iron with water immersion, high humidity, salt spray, copper sulfate, and potassium ferricyanide–nitric acid tests (ASTM International, 2017b). Copper plating out where a drop of copper sulfate solution is applied means iron is still there, and running this test on remaining parts shows whether the treatment failed to remove the iron or iron arrived after treatment.

The fix starts with keeping iron away from stainless steel. Keep dedicated stainless tools, wheels, brushes and fixtures, colour-code them, and switch supports and transport bins to plastic or stainless steel. Re-treat any part touched up or reworked after passivation, and fix an iron detection test from the specification for every lot. Preventing iron from carrying over when cleaning baths, pickling baths and rinse water are reused is also a precaution the standard requires (ASTM International, 2017a).

Hypothesis 2: wrong acid conditions

Look at this hypothesis when bath concentration checks have lapsed for a while, a heater fault has let the temperature drop, or immersion time has been cut to clear a backlog. It also covers a switch from a nitric to a citric process with conditions set only at the specification minimum. Think back to a month when output jumped all at once. Baskets were cycled faster than usual so immersion time shrank, and the bath top-up log has been blank for weeks. Only the lots treated that month show scattered rust spots, with no pattern to where they sit.

Acid dissolves the iron and helps a film with a higher chromium share form on the surface, but the job is finished only when concentration, temperature and time are all right together. The passivation specification sets citric acid at 4 to 10% and varies the minimum time with temperature, giving less guidance on combinations of concentration, temperature and time than it does for nitric acid. In tests varying conditions within that range, the common grade 304L matched nitric acid results after 20 minutes at 4%, but in free-machining 303 some specimens passivated and others did not below 7% or under 60 minutes, and the precipitation-hardening grade 17-4 PH passivated consistently only at 10% for 60 minutes (Enos & Wichhart, 2021). Conditions inside the specification range, in other words, can still fall short for some grades. As iron and other metals dissolve into the bath and build up, the acid loses strength accordingly.

Start by matching the records against the bath. Set the acid concentration analysis, bath temperature log and immersion time for the day the rusted lot was treated next to the conditions in the applied specification, and re-analyse the bath for its current concentration and dissolved iron. Run the specification's verification tests on remaining parts from the same lot, and treat coupons of the same grade under varied conditions to see which conditions pass (ASTM International, 2017b).

Once drifting conditions are confirmed, tie bath control to numbers. Analyse concentration at fixed intervals with a top-up rule, replace the bath when dissolved iron passes a limit, and log temperature and time with a recorder. For each grade, set conditions within the specification range that have passed the verification tests, and do not shorten that time even when work piles up.

Hypothesis 3: grade mismatch

This hypothesis takes the lead when free-machining grades with added sulphur such as 303 or 416, low-chromium martensitic grades or precipitation-hardening grades are treated under the same conditions as 304 or 316. Plants that load parts of several grades into one basket and treat them together are especially prone. In one basket, 304 bolts and 303 nuts went through the same bath together. In the salt spray test the bolts stayed clean while the nuts bloomed with rust spots, and a few had turned dark straight after treatment.

Free-machining grades are awkward because of the inclusions that help machining. 303 and 416 are grades in the specification for free-machining stainless steel bars (ASTM International, 2022). Both are made with at least 0.15% sulphur so that a network of manganese sulphide inclusions forms, and where these inclusions meet the surface they are electrochemically active and become starting points for localised corrosion. Nitric acid passivation of free-machining grades therefore adds an inhibitor such as sodium dichromate to limit damage during treatment (Enos & Wichhart, 2021). In the same study, 416, with chromium as low as 12 to 14%, did not passivate in citric acid. One study explained why pits start around manganese sulphide by chromium depletion around the inclusions, and a rebuttal re-examined the same sample and found no such depletion (Ryan et al., 2002; Meng et al., 2003). Whatever the explanation, the places where inclusions break the surface remain weak points.

Confirm the actual grade from the certificate, and if there is no certificate or a mix-up is suspected, measure chromium, nickel and molybdenum with a handheld analyser. Compare against the other grades in the same basket to see whether the rust is confined to one grade, and check whether the surface darkened right after treatment. In tests using citric acid on free-machining grades, the surface also turned dark blue during treatment, and the discolouration disappeared once an alkaline step was added before and after (Enos & Wichhart, 2021).

In this case, split baskets and conditions by grade. The appendix of the passivation specification gives guidance on choosing treatments by grade (ASTM International, 2017b), so for free-machining and martensitic grades agree with the supplier on a method suited to the grade, such as nitric acid with an inhibitor or an alkaline, acid, alkaline sequence, and confirm it with verification tests. Where the service environment is harsh, review at the design stage replacing the free-machining grade with a standard one.

Hypothesis 4: poor rinsing

Suspect the rinse for parts with blind holes, threads, overlapping plates and narrow gaps, when parts are packed so tightly in a basket that water cannot reach every corner, when rinse tanks have gone unchanged for a long time, or when the final rinse uses tap water alone. A stainless block drilled with several threaded holes is boxed and shipped still holding water after treatment. When the customer opens the box days later, a brown streak runs down from every threaded hole, while the flat faces are clean.

Rinsing matters because if acid and what it dissolved stay on the surface, the treatment does not stop there. The standard requires thorough rinsing after passivation and calls for care that iron is not carried over when cleaning solutions and rinse water are reused (ASTM International, 2017a). In the tests comparing citric and nitric passivation, too, treated specimens were rinsed in flowing deionised water and then dried at once with filtered dry gas (Enos & Wichhart, 2021). Acid solution left in holes and gaps concentrates as the water evaporates, and the iron dissolved in it settles back onto the surface. Chloride in tap water or in a dirty rinse is left behind on drying too. Pitting starts in the presence of aggressive anions such as chloride and grows in an occluded environment that has turned acidic, such as the inside of a narrow hole (Frankel, 1998).

Rust that seems to flow out of holes, threads or overlapping faces fits this hypothesis. Touch pH paper to water draining from the holes of finished parts, and measure the conductivity of the final rinse tank against fresh water. Whether water poured on a rinsed surface breaks up instead of sheeting evenly, and whether a white cloth wipe picks up residue, are also cleanness checks set out in the standard (ASTM International, 2017a). Check the records for how long the parts took to dry and whether they were packed wet.

If rinsing looks short, break it into stages. Set up several stages of flowing or counter-flow rinsing, make the final rinse deionised or purified water, and set its change interval by conductivity. Agitate or spray holes and threads during rinsing so water flows in and out, blow them out with compressed air afterwards and dry at once. Do not pack parts until they are fully dry.

Hypothesis 5: chloride exposure

When parts pass verification tests straight after treatment but rust in service, look at the environment. Coastal plant, spots splashed with de-icing salt in winter, food and hygiene equipment wiped with chlorine sanitisers or hydrochloric acid cleaners, and places touched by process fluids containing chloride all qualify. Take outdoor covers at a plant not far from the sea. Made from 304 and passivated, after a year they show small rust spots scattered over the surface with rust stains spreading below them, darker on the lower parts that rain does not wash.

The passive film is very thin, 1 to 3 nm (Olsson & Landolt, 2003), and chloride breaks through it locally. Whether pits form is set jointly by potential, temperature, chloride concentration and alloy content, and alloying elements such as molybdenum raise resistance to pitting (Frankel, 1998). Passivation cleans the surface so the grade regains its inherent corrosion resistance; it does not lift it any higher, so when the environment exceeds the grade's limit, rust appears even on a well-treated surface. Places where salt builds up through wetting and drying, narrow gaps and warm spots reach that limit first.

First confirm whether the rust came in service rather than right after treatment, and whether the service environment contains chloride. Wipe around the spots with purified water and test the rinse with chloride test strips, and check the SDS of the cleaners and sanitisers in use for chlorine or hydrochloric acid. If parts from the same lot kept indoors are sound, the weight shifts from the treatment to the environment. Looking under a magnifier for pinhole-like pits where spots have been wiped off shows whether the attack has become pitting.

The remedy is to rematch the grade to the environment. Where chloride is heavy, consider a more resistant grade such as molybdenum-bearing 316, wash surfaces where salt builds up with clean water regularly, and design out shapes that hold water or form crevices. Switch to non-chlorine cleaners or require thorough rinsing after use, and for spots where pitting has started, discuss polishing and re-treatment with the supplier.

Hypothesis 6: heat tint left on

This hypothesis fits when welded structures or piping are shipped after passivation alone, when too little backing gas has left the weld root heavily discoloured, or when discolouration has been rubbed off with a wire brush only. A frame welded from stainless steel box section is a good example. It was passivated and installed, and months later rust has formed only along the yellow and blue bands either side of the welds, while faces away from the welds are clean.

Discolouration from welding heat is a thickened oxide film. It is a chromium-rich oxide that gives little protection, and the stainless steel beneath is left as a chromium-depleted layer with lower corrosion resistance. In tests, heat-tinted surfaces were more prone to pitting and crevice corrosion, purple-blue oxides were the weakest, and the critical pitting temperature of a type 316 weld in 0.1% sodium chloride solution could drop from 60 °C to 40 °C (TWI, n.d.-a). Restoring the surface means removing both the oxide and the chromium-depleted layer, and grinding followed by pickling recovers the pitting temperature best; wire brushing or sand blasting is less effective because it generally leaves the depleted layer (TWI, n.d.-b). Passivation dissolves iron from the surface rather than stripping such oxide (ASTM International, 2017a), so passivating over heat tint leaves the weak band in place.

Rust in bands along the welds puts heat tint first in line. Check the colour and width of the tint in pre-shipment photographs or on remaining parts, and confirm from work records the backing gas, how its oxygen was controlled and how the tint was removed. Where the same frame has welds that were ground and pickled and others that were only brushed, compare the rust on the two. Sites that use a colour chart for acceptable discolouration should check against it as well.

If heat tint is the cause, change the process order. Purge the backing gas well before welding so less tint forms in the first place, and remove the tint that does form by fine grinding followed by pickling, or with pickling paste, before passivating (TWI, n.d.-b). If brushes are used, keep them for stainless steel only and do not stop there. After treatment, run the verification tests on the welds as well.

Finding the cause

There is no need to investigate all six hypotheses at once. Rule them out starting with what records and the eye can confirm. Grade certificates and passivation records are on paper, and whether the rust follows the welds, flows from holes or lines up along machining marks is plain from the part. Bath analysis, composition analysis and control treatments take time, so they come next.

The place and timing of the rust point to the cause. Spots lined up along machining marks or tool contact point to iron contamination, bands either side of welds to heat tint, and streaks running from holes and threads to rinsing. Rust confined to one grade within a basket points to the pairing of grade and treatment, and rust scattered across every lot treated in a certain period points to acid concentration, temperature and time. If verification tests passed right after treatment and rust came in service, lean towards chloride exposure.

If that still does not settle it, run control treatments. Split parts from the same lot: treat one group under the current conditions, one in fresh acid under conditions matched to the grade, and one under those conditions plus a deionised final rinse and immediate drying, then put all three through the same verification tests. Only one thing should differ at a time, or there is no telling what stopped the rust. If grades are mixed, run the same comparison separately for each grade.

The final check is real lots. Run the specification's verification tests on the next few lots treated with the revised process, and watch for a set period whether rust is reported again from the customer's site after shipment. The job is done only when passing tests and a clean field record go together.

The hypotheses often overlap. Heavy iron contamination meeting weak acid conditions leaves iron behind, holes that were poorly rinsed collect chloride from tap water as well, and both free-machining inclusions and heat tint give way first in a chloride environment. When several causes appear together, fix what lies inside the treatment process first, iron contamination, acid conditions, grade-specific treatment, rinsing and tint removal, and then look at the service environment, because while the process is unsettled it is hard to tell the environment's share from the treatment's.

Limits and cautions

Acid type, concentration, temperature, time, rinse water quality, and the choice of verification tests and their acceptance criteria differ by grade, applicable specification and customer requirement, so figures follow that specification and the chemical's TDS. For medical, food, semiconductor or pressure equipment parts with their own specifications, do not change the process on floor judgement alone; get approval from the quality engineer and the customer. Whether parts with deep pitting can still be used is for the laboratory and the design engineer to decide.

Take particular care with safety. For nitric acid, citric acid, the hydrofluoric acid mixtures and pastes used in pickling, and dichromate inhibitors, follow the product's safety data sheet, the SDS, for protective equipment, ventilation and waste disposal. Hydrofluoric acid can cause deep injury on skin contact, so never handle it without the first aid preparations the SDS specifies, and run local exhaust when working at nitric acid tanks, which can give off toxic fumes.

Sources

  1. ASTM International. (2017a). ASTM A380/A380M-17, Standard practice for cleaning, descaling, and passivation of stainless steel parts, equipment, and systems. https://store.astm.org/a0380_a0380m-17.html
  2. ASTM International. (2017b). ASTM A967/A967M-17, Standard specification for chemical passivation treatments for stainless steel parts. https://store.astm.org/a0967_a0967m-17.html
  3. ASTM International. (2022). ASTM A582/A582M-22, Standard specification for free-machining stainless steel bars. https://store.astm.org/a0582_a0582m-22.html
  4. Enos, D. G., & Wichhart, D. (2021). Refinement of citric acid passivation methods and comparison to traditional nitric acid based chemistries (SAND2021-12075C). Sandia National Laboratories. https://www.osti.gov/biblio/1890611
  5. Frankel, G. S. (1998). Pitting corrosion of metals: A review of the critical factors. Journal of the Electrochemical Society, 145(6), 2186–2198. https://doi.org/10.1149/1.1838615
  6. Meng, Q., Frankel, G. S., Colijn, H. O., & Goss, S. H. (2003). Stainless-steel corrosion and MnS inclusions. Nature, 424(6947), 389–390. https://doi.org/10.1038/424389b
  7. Olsson, C.-O. A., & Landolt, D. (2003). Passive films on stainless steels—chemistry, structure and growth. Electrochimica Acta, 48(9), 1093–1104. https://doi.org/10.1016/S0013-4686(02)00841-1
  8. Ryan, M. P., Williams, D. E., Chater, R. J., Hutton, B. M., & McPhail, D. S. (2002). Why stainless steel corrodes. Nature, 415(6873), 770–774. https://doi.org/10.1038/415770a
  9. TWI. (n.d.-a). Avoiding heat-tint during welding of stainless steels. TWI Ltd. Retrieved November 2026. https://www.twi-global.com/technical-knowledge/faqs/faq-what-is-heat-tint-and-how-do-i-avoid-it-during-welding-of-stainless-steels
  10. TWI. (n.d.-b). Removing heat-tint from stainless steels. TWI Ltd. Retrieved November 2026. https://www.twi-global.com/technical-knowledge/faqs/faq-how-do-i-remove-heat-tint-formed-during-welding-or-improper-heat-treatment-of-stainless-steels

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.