KALTECKOREA

BlogApplication notes

Why does penetrating oil swell rubber seals and belts?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Maintenance Aids

Replacing a swollen seal or belt with the same part is the usual response, but rubber swells because liquid has soaked into it, so if the way the spray is used stays the same, the new part tends to swell as well. What actually lies behind it can be solvent and mineral oil that do not suit the rubber, overspray and pooling, an oil-sensitive rubber type, long contact time or cleaning that was missed or wrong, and sometimes two or more at once.

Background

A few days after penetrating oil was sprayed generously on a rusted bolt, the oil seal lip on the gearbox beside it has swollen and gone soft, and the V-belt below has a tacky surface and squeals as it slips. The bolt came free, but now the seal leaks oil and the belt needs replacing.

The cost is more than the parts. A swollen seal goes soft at the lip and lets oil past, and a belt slips, transmits less power and wears faster. Unplanned stops and replacements follow, and swapping in the same part without knowing the cause repeats the same story. Rubber that swells almost always softens with it, and with excessive swell it loses abrasion and tear resistance and can be extruded into gaps under high pressure (Parker Hannifin, 2007).

Rubber swells because liquid soaks into it. Its crosslinks, the network that ties the rubber's molecular chains together, keep it from dissolving, but liquid molecules work into the gaps and stretch the network. Swelling stops where the pull of the liquid to get in is balanced by the stretched network trying to pull back (Flory & Rehner, 1943). The closer the solubility parameters of rubber and liquid, values that describe how strongly their molecules attract each other, the more the liquid swells that rubber (Hansen, 2007; Jing & Liu, 2024).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: confirm from the drawing or the part marking what rubber the swollen seal and belt are made of, then set the composition section of the penetrating oil's safety data sheet, the SDS, beside what its technical data sheet, the TDS, says about rubber compatibility.

Hypothesis 1: unsuited ingredients

When penetrating oil is used near rubber parts, suspect its composition first. A penetrant is defined as a lubricant designed to loosen metal parts bonded together by rust or oxidation, and is regulated as a product category with a ceiling on volatile organic compound content (CARB, 2022). In other words the product may combine oil with volatile solvent, and the kind and amount of solvent differ from product to product. One such spot is a coupling bolt seized with rust, right next to a pump's shaft seal and a rubber coupling element. Liquid aimed at the bolt wets the area around the seal and the rubber element as well.

How much a given rubber swells depends heavily on the liquid. The aniline point of a hydrocarbon liquid, the lowest temperature at which it mixes completely with an equal volume of aniline, is lowest for aromatics and highest for paraffins, and is used to estimate aromatic content (ASTM International, 2023). The lower an oil's aniline point, the more severe its swelling action. Aromatic oils can make rubbers such as nitrile rubber, NBR, keep swelling without reaching equilibrium, and NBR resists aliphatic hydrocarbons and mineral oil but not aromatics, chlorinated solvents or polar solvents such as ketones (Parker Hannifin, 2007). Experiments have also shown NBR swelling strongly in liquids whose solubility parameters are close to its own (Jing & Liu, 2024).

The check begins with the composition list. Look in the SDS composition section for aromatic solvents, chlorinated solvents and ketones, and ask the supplier whether there are data on the base oil's aniline point and on rubber compatibility tests. If there are none, soak a spare part or an offcut of the same rubber in the liquid and see how its volume, mass and hardness change. A standard test method measures how well rubber withstands a liquid in just this way, by property changes before and after immersion (ASTM International, 2021).

If the composition proves unsuitable, set aside a separate product for use near rubber. Choose one without aromatic or chlorinated solvents, or one for which the supplier can show compatibility test data with that rubber, and write into the maintenance standard that only that product is kept at equipment with many rubber parts. Even with the new product, it is safer to run a soak test on a spare offcut before use.

Hypothesis 2: overspray and pooling

This hypothesis arises when a wide-fan nozzle wets several bolts at once, when liquid sprayed on upper bolts runs down, or when the same spot is sprayed again and again because it will not free. The run-off collects in low, hollow places such as the groove under a seal lip, the floor of a belt guard or the pulley grooves. Spraying down from above to free the hold-down bolts on a motor base is such a case. The liquid wets the bolts, runs on and drips onto the belt, and a thin film of oil lies in the bottom of the pulley groove and under the guard.

Pooling matters because of the difference between a film that wets and dries and a part that sits in liquid. A thin coat shrinks as the solvent evaporates, but pooled liquid keeps the rubber wet as in an immersion test, and absorption continues the whole time. Exposed surface matters too. Rubber pressed into a groove has less surface in contact with the liquid and swells considerably less than in the free state, and in immersion tests rings with smaller cross-sections swelled more than larger ones (Parker Hannifin, 2007). That is why the exposed tip of a seal lip and the thin outer layer of a belt tend to swell first.

Follow the traces. Look for wet tracks running down from where the spray went, black lines where dust has stuck, and oil pooled in hollows, and see whether the swollen part sits below that flow. Compare it with the same rubber part elsewhere on the equipment, out of the flow, by pressing with a fingernail or with a durometer, and it becomes clear whether the swelling follows the path of the run-off.

If pooling is the cause, change how the spray goes on. Feed small amounts into the bolt thread only through a thin straw nozzle, cover seals and belts below with a cloth or a board before spraying, and wipe up run-off on the spot. When working above a belt drive, take the belt off or cover it with the guard, and clear oil pooled in hollows once the job is done.

Hypothesis 3: oil-sensitive rubber

If only certain parts swell when the same product was used the same way, look at their rubber. The typical case is a rubber chosen to withstand water, steam, brake fluid or weather, sitting where oil reaches it. Rubber gaskets at cooling water pipe joints, and anti-vibration mounts or roller covers made of natural rubber, are examples. A nitrile seal and the gasket on the cooling water hose next to it take the same spray on the same day; the seal is fine, but the gasket has visibly swollen.

Rubbers differ widely in how they stand up to oil. Ethylene propylene rubber, EPDM, and butyl rubber resist water, steam and polar solvents but are not compatible with mineral oil products. NBR resists oil better the higher its acrylonitrile content, but its elasticity and resistance to compression set suffer, so a medium content is usual (Parker Hannifin, 2007). The automotive rubber classification system grades rubbers by their volume swell limit in oil, and its lowest grade has no swell requirement at all (ASTM International, 2018). Even within one rubber type, the compound makes a difference. In natural rubber, the amount of aromatic hydrocarbon taken up differed with the crosslinking system (Unnikrishnan & Thomas, 1994).

Find the part's material in the drawing, the parts list or the purchase specification. If the specification carries a rubber classification code, the oil swell grade can be read from it. Without records, ask the parts supplier for the material, and soak spare parts separately in the penetrating oil used and in a reference mineral oil to compare. Recording hardness and dimensions against an unswollen part of the same kind also makes it possible to judge later whether a material change worked.

Once the rubber is confirmed as oil-sensitive, change one of the two. Where oil cannot be kept off, change the part specification to an oil-resistant material, checking with the parts supplier that it still meets the water, heat and weather conditions the original rubber had to withstand. Where the part cannot be changed, do not use penetrating oil around it, or limit its reach, for example by brushing it onto the thread only.

Hypothesis 4: long contact time

Penetrating oil is often left overnight or over a weekend, on the common advice to give it time to soak in. Freeing a seized bolt over several days with a fresh spray each day, or spraying routinely as rust protection, also lengthens contact time. Spray a seized flange bolt on Friday afternoon, come back on Monday morning to free it, and the rubber boot beside the bolt is thicker than it was on Friday.

Liquid enters rubber from the surface inwards by diffusion, the spreading of molecules towards lower concentration. The rate depends on factors such as the rubber's structure, the size of the liquid's molecules and temperature (George & Thomas, 2001), and the amount absorbed grows with time and levels off as it nears equilibrium. In diffusion theory the time to reach equilibrium scales with the square of thickness (Crank, 1975), so thin lips and the outer layer of a belt fill up quickly even with brief contact while the thick body follows slowly. Some rubbers swell in a short test and then shrink after long exposure, so the swell from a 70-hour immersion test may not be the final state (Parker Hannifin, 2007).

This hypothesis is sorted out by measuring again over time. Measure the swollen part's thickness or lip diameter and its hardness now, then wipe the liquid off and measure at the same spot again over several days. If dimensions and hardness come back a good way as volatile components such as the solvent leave, it was temporary swelling from physical soaking; if they do not, or the rubber has cracked or turned tacky, treat it as permanent damage involving chemical change. Rubber's loss of properties can be temporary, from liquid soaking in alone, or permanent, from chemical change (Parker Hannifin, 2007).

When long contact looks responsible, keep the contact on the bolt and take it off the rubber. While giving the oil time to soak in, cover rubber parts or wipe around them, and feed the bolt small amounts several times instead of a large amount at once. For a job spread over days, put wiping the rubber side each day into the work sequence, and handle rust protection separately with a rust preventive rather than a penetrant.

Hypothesis 5: poor cleaning

Once the bolt is free, it is easy to treat the job as finished and leave the remaining oil where it is. The opposite also happens, where a strong cleaning solvent is sprayed liberally on the rubber to get it clean. Both are cases where the cleaning step was missed or wrong. A conveyor goes back into service after maintenance with the area round the bolts and the belt edge still glistening, and a few weeks later only that belt edge has gone soft.

Residual oil becomes a reservoir that keeps feeding liquid to the rubber. After the solvent has evaporated, the oil remains in contact with the rubber, and absorption continues as long as that contact lasts. Wrong cleaning causes trouble too. A liquid can dissolve out the rubber's plasticiser, the ingredient added to keep it soft, and that rubber shrinks once the liquid leaves and it dries. Shrunken rubber usually hardens and pulls away from the sealing surface, leaving a leak path, so shrinkage is more critical than swell, and for moving seals more than 3 to 4% shrinkage can be serious (Parker Hannifin, 2007).

Touch is the first check. If the area round the seal and the belt surface is glossy or tacky, oil remains, and rubbing with a dry white cloth shows roughly how much. Find in the maintenance records and work orders whether there was a cleaning step and, if so, what cleaner was used. If a part has shrunk and hardened rather than swollen, look at a cleaner that leached out the plasticiser.

Put a cleaning step at the end of the work sequence. After the bolt comes free, first wipe the oil off rubber parts and their surroundings with a dry cloth, then clean what remains with a cleaner the rubber part's supplier allows. Do not spray strong solvent directly on rubber. Judge belts and seals that have already swollen on measurements repeated over time, and replace them if dimensions and hardness do not come back.

Finding the cause

Clear the five hypotheses starting with what documents and the eye can confirm. The rubber material and the spray's composition are in the drawing and the SDS, and run-off tracks and leftover oil are visible right at the equipment. Soak tests and measurements repeated over time take days, so they come after.

The first clue is which parts swelled. If, among the rubber the spray reached, only a certain material swelled, look at an oil-sensitive rubber type; if parts swelled regardless of material but only below the flow, look at overspray and pooling. If even oil-resistant material swelled, suspect incompatible composition, especially aromatic or chlorinated solvents.

Next is the form of the swelling and how it changes. If dimensions come back a few days after wiping, the swelling was temporary, and the answer lies in shortening contact time and removing leftover oil. If they do not, and cracks or tackiness appear, treat it as permanent damage from an unsuitable composition or rubber type. A part that shrank instead of swelling points to the cleaner.

If that still does not settle it, run control trials. Soak several spare offcuts of the same rubber for the same time in the penetrant in use, in another product and in a reference mineral oil, leaving one unsoaked. Measure volume, mass and hardness the same way when they come out, and again after a few days of drying. Vary only the liquid or only the time in each comparison, or there is no telling which factor caused the swelling. The final check is that, after a period of use with the new product and method, the dimensions and hardness of new parts in the same position hold.

The hypotheses often overlap. An unsuitable composition running down and pooling, an oil-sensitive rubber sitting below it, and leaving it uncleaned for a long time can all be part of one job. In such cases, put right what is easiest to change first, the spraying method, shielding and wiping, and if parts still swell after that, change the product and the rubber material, because while the working method is unsettled the effect of a material change cannot be compared fairly.

Limits and cautions

How far a rubber swells in a given liquid differs by compound even within one rubber type, so compatibility decisions follow the parts supplier's data and a soak test with the actual liquid. Figures such as the shrinkage limit for moving seals are only general guidance, and for safety-related seals such as those in brakes, hydraulic systems and pressure vessels, do not return parts to service on floor judgement alone; follow the equipment manufacturer's criteria.

Safety matters too. Penetrating oils and cleaning solvents are usually flammable, so ventilate according to the product's SDS, keep away from sparks and hot surfaces, and protect skin and eyes. When spraying or wiping near belt drives and rotating parts, always stop the equipment, isolate the power and apply locks and tags first (OSHA, n.d.).

Sources

  1. ASTM International. (2018). ASTM D2000-18, Standard classification system for rubber products in automotive applications. https://store.astm.org/d2000-18.html
  2. ASTM International. (2021). ASTM D471-16a(2021), Standard test method for rubber property—Effect of liquids. https://store.astm.org/d0471-16a.html
  3. ASTM International. (2023). ASTM D611-23, Standard test methods for aniline point and mixed aniline point of petroleum products and hydrocarbon solvents. https://store.astm.org/d0611-23.html
  4. California Air Resources Board [CARB]. (2022). The California consumer products regulations (California Code of Regulations, Title 17, Sections 94507–94517). https://ww2.arb.ca.gov/sites/default/files/2023-01/Consumer%20Products%20Final%20Reg%20Order_1-20-2023.pdf
  5. Crank, J. (1975). The mathematics of diffusion (2nd ed.). Clarendon Press.
  6. Flory, P. J., & Rehner, J. (1943). Statistical mechanics of cross-linked polymer networks II. Swelling. The Journal of Chemical Physics, 11(11), 521–526. https://doi.org/10.1063/1.1723792
  7. George, S. C., & Thomas, S. (2001). Transport phenomena through polymeric systems. Progress in Polymer Science, 26(6), 985–1017. https://doi.org/10.1016/S0079-6700(00)00036-8
  8. Hansen, C. M. (2007). Hansen solubility parameters: A user's handbook (2nd ed.). CRC Press.
  9. Jing, Y., & Liu, G. (2024). Systematic investigation on the swelling response and oil resistance of NBR using the prediction models determined by the modified Flory–Huggins interaction parameter. Polymers, 16(19), 2696. https://doi.org/10.3390/polym16192696
  10. Occupational Safety and Health Administration [OSHA]. (n.d.). Control of hazardous energy (lockout/tagout). U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/control-hazardous-energy
  11. Parker Hannifin. (2007). Parker O-ring handbook (ORD 5700, 50th anniversary ed.). Parker Hannifin Corporation, O-Ring Division.
  12. Unnikrishnan, G., & Thomas, S. (1994). Diffusion and transport of aromatic hydrocarbons through natural rubber. Polymer, 35(25), 5504–5510.

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.