KALTECKOREA

BlogApplication notes

Why does plating show pits?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Coatings & Surface Treatments

Adding more wetting agent is the usual response to pits in plating, but a pit forms where a bubble or a foreign body stops metal from building up, so pits return as long as whatever held it there remains. What actually lies behind them can be too little wetting agent, organics in the bath, particles in the bath, a flawed base metal or poor agitation, and sometimes two or more at once.

Background

Turn a part fresh from bright nickel plating under a light and you see pinpoint holes scattered across an otherwise smooth face. These small holes, which the shop calls pits, fail visual inspection at once, and saving the part means stripping the plating and starting again. It is not only about looks. A hole in the plating can give corrosive agents a path to the base metal beneath, so a small blemish on the surface can later grow into rust or blistering (Dini, 1993).

A pit is defined as a small depression or cavity produced in a metal surface during deposition or by corrosion, and a process specification for nickel plating lists pitting among the defects to look for in visual inspection (NASA, 2026). Why pits form in nickel plating and how to prevent them has been studied since the 1920s (Macnaughtan & Hothersall, 1928).

The principle is simple. Metal builds up only where the solution reaches, so anything that covers one spot on the surface leaves that spot empty while the area around it thickens, and a hole remains. Pits in nickel plating are mainly attributed to bubbles of hydrogen or other gases; most bubbles do not stick and leave, but bubbles were reported to stay attached at irregular spots such as scratches, small nodules and foreign particles lodged on the surface (Cymboliste, 1936). So what makes a pit is less the bubble itself than the condition that holds a bubble or a foreign body in place.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: keep the pitted parts, mark which faces and spots the pits gather on, and compare that day's bath analysis, current density, temperature, agitation and additive records with the control ranges in the plating chemistry's technical data sheet, the TDS.

Hypothesis 1: low wetting agent

Nickel plating solutions carry a wetting agent, a surfactant that helps bubbles leave the surface easily. Wetting agent is lost on the parts as they leave the tank and can also drop when the bath is carbon-treated to remove organics, so when replenishment falls behind, this hypothesis comes to the front. Think of the end of a week with heavy output. Additions were made on the usual schedule, yet round, smooth holes appear in rows along the edges and corners of flat parts. Every part on the same rack has holes in similar places.

On the part, which is the cathode, hydrogen ions turn into hydrogen gas alongside the reaction that deposits nickel, so small hydrogen bubbles form all the time (Zhao et al., 2019). Buoyancy pulls a bubble away, but at the line where the bubble meets the surface, surface tension holds it. In experiments that watched hydrogen bubbles on a nickel electrode directly, once this contact line was pinned in place the bubble left only after growing until its contact angle reached a limit (Demirkır et al., 2024). In one study, some hydrogen stuck firmly to the electrode as bubbles during nickel plating and formed pits at the electrode edges; adding sodium dodecyl sulfate, a long-chain sulfate surfactant, let the bubbles leave on their own with no visible pitting (Tsuru & Takemoto, 2005). With too little wetting agent, bubbles stay longer and grow larger, and meanwhile nickel grows around them and leaves each bubble site as a round hole.

Whether there is enough wetting agent can be measured through the surface tension of the solution. Take a sample, measure it with a tensiometer and compare it with the supplier's range; the Wilhelmy plate method, which measures the pull on a thin plate dipped in the liquid, was used to assess an anti-pitting additive in nickel plating solutions (Salakhova et al., 2023). Without an instrument, lay the wetting agent additions beside the charge passed, the ampere-hours, and see whether additions kept pace with it. Pits that are round, smooth inside and gathered along edges give this hypothesis more weight.

If surface tension sits above the range, bring the wetting agent back into the supplier's range, and from then on add it little and often in step with ampere-hours rather than in large doses. Put a wetting agent analysis and top-up after every carbon treatment into the work instructions. For tanks stirred with air, confirm with the supplier that the wetting agent is a low-foam type. After topping up, rack the same parts again and see whether the pits disappear.

Hypothesis 2: organics in the bath

Besides the additives put in on purpose, organics build up slowly in a plating solution. Oil carried in on poorly degreased parts, residues left as brighteners break down under current, and substances leached from new hoses or tank linings are examples. Consider the weeks after a new part, formed with plenty of press oil, joins the line. Topping up wetting agent does not reduce the pits, the holes sit in different places on each part, and an oil film floats on the degreasing tank.

Organics make pits in two ways. One is through the surface. A spot with oil left on it repels water, and such water-repellent films are found by flooding a cleaned part with water and watching for the water film to break (ASTM International, 2021). A water-repellent surface is also one on which bubbles spread and stick, so they find it hard to leave (Zhao et al., 2019). The other is during plating. Organic compounds adsorbed on the surface, along with finely dispersed oxides, hydroxides and sulfides, are described as seeds of defects in the deposit that can leave holes (Dini, 1993). So organic contamination keeps making sites where bubbles stick, however much wetting agent is added.

Start with the parts. Take a few parts after degreasing and pickling, just before the plating tank, flood them with water and see whether the film covers them evenly without breaking. Removing such films is the very purpose of cleaning before plating, so if the water film breaks, look again at degreasing and rinsing conditions first (ASTM International, 2025). Check the solution with a Hull cell, a small test cell that plates one panel across a span from low to high current density in a single run (DIN, 2016). Plate one panel with the tank sample as it is and another with the same sample after a small activated carbon treatment, then compare the pits side by side.

If the pits vanish on the carbon-treated panel, the cause is organics in the solution. Agree a full-tank carbon treatment with the supplier, and afterwards analyse and restore the wetting agent and brightener removed along with the organics. If oil is coming in on the parts, the tank will soon load up again after treatment, so rework degreaser concentration and temperature, oil skimming and the number of rinse stages at the same time. Right after a change of hose or lining, confirm with the supplier that the material suits the solution.

Hypothesis 3: particles in the bath

Small particles float in a plating solution when the filter is clogged or its flow has dropped, when an anode bag tears and anode residue escapes, when dust drifts in from the roof or a polishing area, and when the pH rises and metal hydroxides precipitate. A tank whose anode bags are overdue for a change shows this. Lift a part and the upward-facing surfaces carry holes mixed with small bumps that catch the fingertip, while downward-facing surfaces are fairly clean.

First, a particle masks the surface. One that settles on a part masks that spot so metal cannot cover it, and particles that settle out of the solution onto the surface are listed with slag, oxides, abrasive and dirt as seeds that start holes (Dini, 1993). A foreign body lodged on the surface is also a place where bubbles stay. The bubble study cited earlier named foreign particles lodged on the surface, along with scratches and nodules, as reasons bubbles stick (Cymboliste, 1936). A particle that is simply covered over becomes a bump, and metal growing around a bubble attached to a particle leaves a hole, so under this hypothesis pits and rough bumps can appear together.

Dip a tank sample into a clear beaker and hold it to the light, and floating particles show. Filter the sample through filter paper, keep the residue and, if needed, have the supplier or a laboratory analyse it to narrow down where it came from. Check the pressure drop across the filter, the turnover per hour, and the condition and change records of the anode bags. Counting pits on the upward- and downward-facing surfaces of a part shows whether settling particles are to blame.

If particles look to be the cause, put filtration right first. Change clogged filters, set the turnover to the supplier's recommendation, and replace torn anode bags. For sludge on the tank floor, transfer and filter the solution into another tank, then clean the tank. If a rise in pH formed hydroxides, bring the pH back into range, and if dust is the source, rework tank covers and the layout of the shop.

Hypothesis 4: flawed base metal

If the solution and conditions are unchanged but pits come only on parts from one material lot, one casting or one polishing job, look at the base metal. Castings with internal pores such as zinc die castings, steel with inclusions or laps at the surface, steel pickled too long, and polished faces with abrasive pressed into them are examples. Suppose castings from two suppliers hang on the same rack on the same day. One set is clean while the other shows holes, and the holes recur at similar spots on parts of the same shape.

While the deposit is thin, its porosity, the number of holes in it, depends largely on the condition of the base metal surface, and inclusions in the base metal such as slag, oxides and sulfides, or carbon particles left on over-pickled steel, become defects that plating does not cover. Where the base metal has pores, as castings do, solution trapped in a pore can later seep out and cause trouble even if the deposit itself has no hole. Abrasive or polishing residue left embedded in the surface acts as the same kind of seed (Dini, 1993). Polishing can also expose pores lying near the surface, so if pits increased after polishing, suspect this hypothesis.

The clue lies in the base metal before plating. Examine unplated parts from the same lot under a magnifier for holes, streaks or embedded abrasive already present. Cut one pitted part through a pit and polish the section, and it shows whether the hole began within the deposit or at the base metal surface. A dead-end hole ending inside the deposit and a hole running down to the base metal are classed as different defects, so a hole rising from a pore or an inclusion in the base metal confirms this hypothesis (Dini, 1993). Grouping pits by material lot and supplier shows where they cluster.

If base metal flaws are confirmed, work on the steps before plating rather than plating itself. Return the defective lot to the material supplier with samples and section photographs, and for castings reduce stock removal in polishing or agree a different polishing method with the supplier so pores are not opened. For steel, give pickling only as long as it takes to lift the scale, to avoid over-pickling. Where the flaws are small and scattered, an added underlayer to cover them can be reviewed with the plating chemistry supplier.

Hypothesis 5: poor agitation

Suspect agitation when holes in the air sparger clog so air boils up on one side only, when the drive that rocks the cathode bar stops, when pump circulation weakens, or when a new part with many recesses or downward-opening holes is racked. Picture a line restarted after winter maintenance. Air rises briskly at one end of the tank while the far end is calm, and only parts racked at that end have holes, gathered on the inner faces of their recesses.

Buoyancy is not the only force that pulls a bubble off the surface. Liquid flowing past the electrode adds a force that sweeps bubbles away, and imposing flow is listed as a main way to reduce bubbles on electrodes (Angulo et al., 2020). In still liquid, bubbles therefore stay attached until they grow large. Porosity in deposits is also described as varying with the degree of agitation, along with solution composition, additives and current (Dini, 1993). The inner faces of recesses and the inside of holes opening downwards are hard for flow to reach and offer bubbles no way out, so even in one tank pits gather in such places.

Look first from above the tank at whether agitation is even. With air agitation, compare the strength of the bubbles rising along the length of the tank, and check blower pressure and clogged sparger holes. Check that the cathode rocker moves with its full stroke and speed and that circulation pump flow matches the records. If pits gather only in one zone of the tank, one position on the rack or the recessed faces of the part, give this hypothesis weight. Rack the same part facing another way, and you see at once whether the pits move with it.

For an agitation problem, clear blocked air pipes and reset the spacing and direction of the holes so air spreads evenly through the tank. Use clean, oil-free air for air agitation. Repair a stopped cathode rocker, and redesign racks so parts with many recesses hang in a direction that lets bubbles escape upwards. After any change to agitation, look at the wetting agent and foam again as well.

Finding the cause

Five hypotheses do not mean five separate investigations. Rule them out starting with what is easy to measure. Wetting agent records and surface tension, filter pressure and anode bags, and the state of agitation can all be checked today without stopping the line. Hull cell tests and cross-sections take longer, so they come next.

The first clue is where the pits are. Round, smooth holes at similar places along the edges and corners of every part on a rack point to wetting agent and bubbles, and holes mixed with bumps on upward-facing surfaces point to particles in the bath. Pits gathered in one zone of the tank or in the recesses of a part point to agitation, and pits recurring at the same spots only in one material lot or casting point to base metal flaws. If the spots differ from part to part and topping up wetting agent changes nothing, lean towards organic contamination.

Next is the shape of the hole. In a section cut through a pit, a hole whose bottom reaches the base metal with a pore or inclusion there points to the base metal, and a hole that starts within the deposit with a small particle at its bottom points to particles. A round hollow within the deposit with neither a particle nor a base metal flaw is read as the mark of an attached bubble, so look at what holds bubbles in place: wetting agent, organics and agitation.

If that still does not settle it, run control trials. Plate a well-polished, thoroughly cleaned test panel on the same rack as the problem parts. If the panel pits too, the cause lies with the solution or agitation; if the panel is clean and only the parts pit, it lies with the base metal or cleaning before plating. If it is the solution, plate Hull cell panels in turn from the sample as it is, a carbon-treated sample and a sample with added wetting agent, and see which treatment removes the pits. Change only one thing at a time, or there is no telling what worked, and afterwards count pit rejects per the same number of parts on the same basis as before.

The hypotheses can overlap. Irregular spots such as particles and scratches hold bubbles (Cymboliste, 1936), so in a bath with particles, too little wetting agent makes pits form all the more easily. Removing organics with activated carbon can also lower wetting agent, so fixing one thing can bring on another hypothesis. In such cases, first put right what removes the sites where bubbles stick, such as filtration and cleaning, and then set the wetting agent and agitation that pull bubbles away.

Limits and cautions

Suitable wetting agent concentration and surface tension, filter turnover, carbon dose and agitation strength differ by solution, such as Watts nickel, sulfamate nickel, bright nickel, acid copper and zinc, so numeric decisions follow the solution's TDS and the supplier's guidance. Whether to rework a pitted part or strip and replate it is set by the appearance criteria in the drawing and the customer specification, and parts where corrosion or sealing matters should not be released on floor judgement alone; get the quality engineer to confirm.

Safety matters too. Nickel and its compounds are classed as a potential occupational carcinogen, can cause sensitisation dermatitis on skin contact, and enter the body by inhalation, ingestion and skin or eye contact (NIOSH, n.d.). When sampling the solution or adding activated carbon, follow the product's safety data sheet, the SDS, for gloves, eye protection and ventilation, and handle carbon powder so it does not become airborne. Clean tanks and transfer solution only with the power off and locked out.

Sources

  1. Angulo, A., van der Linde, P., Gardeniers, H., Modestino, M., & Fernández Rivas, D. (2020). Influence of bubbles on the energy conversion efficiency of electrochemical reactors. Joule, 4(3), 555–579. https://doi.org/10.1016/j.joule.2020.01.005
  2. ASTM International. (2021). ASTM F22-21, Standard test method for hydrophobic surface films by the water-break test. https://store.astm.org/f0022-21.html
  3. ASTM International. (2025). ASTM B322-99(2025), Standard guide for cleaning metals prior to electroplating. https://store.astm.org/b0322-99r25.html
  4. Cymboliste, M. (1936). The formation and growth of pits in electrodeposited metals. Transactions of The Electrochemical Society, 70(1), 379–396. https://doi.org/10.1149/1.3493917
  5. Demirkır, Ç., Wood, J. A., Lohse, D., & Krug, D. J. (2024). Life beyond Fritz: On the detachment of electrolytic bubbles. Langmuir, 40(39), 20474–20484. https://doi.org/10.1021/acs.langmuir.4c01963
  6. Deutsches Institut für Normung [DIN]. (2016). DIN 50957-1:2016-02, Testing of electrolytes used for electro-deposited metallic coatings — Part 1: Standard Hull cell. https://www.dinmedia.de/en/standard/din-50957-1/244354430
  7. Dini, J. W. (1993). Electrodeposition: The materials science of coatings and substrates. Noyes Publications.
  8. Macnaughtan, D. J., & Hothersall, A. W. (1928). The causes and prevention of pitting in electrodeposited nickel. Transactions of the Faraday Society, 24, 497–509. https://doi.org/10.1039/TF9282400497
  9. National Aeronautics and Space Administration [NASA]. (2026). Process specification for electrodeposited nickel plating (PRC-5004 Rev. E). Lyndon B. Johnson Space Center. https://www.nasa.gov/wp-content/uploads/2026/07/prc-5004-rev-e-for-signature.pdf
  10. National Institute for Occupational Safety and Health [NIOSH]. (n.d.). NIOSH pocket guide to chemical hazards: Nickel metal and other compounds (as Ni). CDC. Retrieved November 2026. https://www.cdc.gov/niosh/npg/npgd0445.html
  11. Salakhova, R. K., Tikhoobrazov, A. B., & Smirnova, T. B. (2023). Study of surface phenomena in nickel-plated electrolytes using a K-100 tensiometer. Industrial Laboratory. Diagnostics of Materials, 89(2), 39–44. https://doi.org/10.26896/1028-6861-2023-89-2-i-39-44
  12. Tsuru, Y., & Takemoto, H. (2005). Evaluation of wetting agents by means of the buoyancy caused by hydrogen bubbles attached to electrode during nickel electroplating. Journal of The Surface Finishing Society of Japan, 56(1), 41. https://doi.org/10.4139/sfj.56.41
  13. Zhao, X., Ren, H., & Luo, L. (2019). Gas bubbles in electrochemical gas evolution reactions. Langmuir, 35(16), 5392–5408. https://doi.org/10.1021/acs.langmuir.9b00119

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.