Jonghwan Moon
Product group
Water & Waste Treatment

Mixing harder and longer to break up lumps is the usual response, but a grain once coated in gel barely dissolves however long it is stirred, and hard mixing cuts the chains that have already dissolved. What actually lies behind the lumps can be powder added too fast and poorly dispersed, too little or too much mixing, too short an ageing time, make-up water with hardness and chlorine, or solution stored too long, and often two or more at once.

Background

Look into the make-down tank and translucent grains are floating in otherwise clear solution, with jelly-like lumps lying on the bottom. Sticky masses catch on the strainer in front of the dosing pump, and although the dose has not changed, the floc in the flocculation tank is smaller and weaker than before. The operator runs the mixer longer, and when that fails, empties the tank and makes the batch again.

Lumps cost more than wasted product. Undissolved lumps clog pipes and dosing equipment, and polymer trapped inside them passes through without treating any water (Sojka et al., 1998). Under-dissolved solution needs a larger dose to do the same work. In one study, solution aged only one hour needed about 75% more polymer than an optimally prepared solution to give the same flocculation performance (Owen et al., 2002). Weaker flocculation clouds the clarifier overflow and carries through to sludge dewatering.

Polymer flocculants used in water treatment are mostly polyacrylamides, very long chains with molecular weights from about one million to thirty million (Xiong et al., 2018). Such chains do not go straight into solution; they take up water, swell, and then dissolve as the entangled chains come free one by one. If the surface of a powder grain takes up water too quickly, that surface becomes a gel layer that keeps water from reaching the inside, and the resulting lumps are called fish eyes on site because of how they look (Sojka et al., 1998). So lumps mostly come from the conditions in the first few seconds of make-down and in the hours that follow.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: write down how and how fast the powder is added, mixing time and speed, ageing time, where the make-up water comes from and the date each batch was made, and compare them with the make-down concentration and preparation conditions in the flocculant's technical data sheet, the TDS.

Hypothesis 1: powder added too fast

Lumps form readily on days when the automatic make-down unit is down and polymer is dissolved by hand, where powder is shaken from the bag over the tank, and where powder goes in first and water after. Powder that has taken up moisture and caked in the bag gives the same result. At the start of a shift, an operator tips a whole bag of powder into a half-filled tank at once and switches the mixer on. The powder swirls on the surface in white islands, slowly sinks, and an hour later the solution is full of pea-sized clear grains.

The moment a lump forms is the moment the grains first meet water. When grains take up water while touching each other, the faces in contact turn to gel together and become one mass, and the gel layer on its outside keeps water away from the dry powder inside. Lumps formed this way stay undissolved and clog pipes and dosing equipment. That is why guidance from a US Department of Agriculture laboratory stresses always adding powder slowly to fast-moving water and never pouring water onto powder (Sojka et al., 1998). The Australian drinking water guidelines likewise say to mix the polymer with water through a well-designed eductor, a device in which the water stream draws in the powder and scatters it, so that lumps of undissolved polymer do not form (NHMRC, n.d.). When each grain is wetted on its own, any gel forms only around that grain, and the whole grain dissolves evenly.

What to check is how it looks at the moment of addition. See whether the powder clumps into islands on the surface, whether wet powder has stuck and hardened around the inlet, and whether water pressure and feed rate at the eductor or powder feeder match their settings. When a bag is opened, see whether the powder pours as fine dust or clumps when squeezed in the hand. Strain the solution through a fine sieve and look at the gel grains left behind; grains with a clear outside and a dry white core are typical of this hypothesis.

The fix is to change how it goes in. Feed powder into the water stream a little at a time through an eductor or powder feeder, and if it must be dissolved by hand, start the mixer first and sprinkle the powder slowly into water that already has a vortex. Keep to the order of water first and powder after, and wipe off wet powder stuck around the inlet every day. Store powder sealed and dry, and do not use powder that has already caked. Liquid products with the polymer dispersed in oil also need suitable mixing at the point where they enter the water (Sojka et al., 1998).

Hypothesis 2: wrong mixing energy

Question the mixing energy after mixer blades have worn or the motor was changed, when the batch moved to a bigger tank but the mixer stayed the same, or, the other way round, when high-speed mixing runs for hours to break lumps. In a tank with weak mixing, grains sink to the bottom and collect in one place; gel piled in the bottom corners while the solution near the surface looks thin points this way. There is an opposite scene too. The morning after a night of high-speed mixing to get rid of lumps, the solution is clear and smooth, yet the floc in the flocculation tank has become smaller.

Mixing does two jobs: it keeps wetted grains suspended in the water, and it keeps renewing the water around each grain to carry dissolved polymer away. With weak mixing, grains settle on the bottom and stick to each other, and the stuck grains become gel lumps as described above. Strong mixing brings a different problem. In tests at different mixing intensities, the viscosity and flocculation activity of polyacrylamide solutions fell as mixing went on and levelled off at limiting values set by the mixing intensity, and light scattering confirmed that the molecular weight had actually dropped (Scott et al., 1996). The long chains had been cut. In tests dissolving powdered anionic polyacrylamide, each molecular weight likewise had its own best mixing speed (Li et al., 2023). That is why stirring hard to break up lumps tends to leave the lumps and lose performance.

Judge mixing energy by eye and from records together. While mixing, see whether grains are lifted from the very bottom and kept moving, and whether gel collects in the corners or under the mixer shaft, and compare mixer speed, blade condition and running time with the design conditions. If overmixing is suspected, take solution from the same batch early and late in mixing and compare its viscosity, or compare performance in a beaker flocculation test, the jar test, run under identical conditions. If viscosity and performance fall together over time, the chains are being cut.

If mixing is too weak, replace worn blades and check with the equipment supplier that the mixer suits the tank size. If it is too strong, stop trying to break lumps by mixing; mix hard only during initial wetting, then stir slowly while it dissolves, just enough to keep grains from settling. Put the high-speed stage on a timer, and strain out lumps that have already formed or discard that batch. Recirculation and high-speed transfer pumps can also cut chains, so check the type of pump that moves the solution as well.

Hypothesis 3: ageing too short

Check the ageing time in seasons when demand rises and the make-down tank empties fast, in units that dissolve and dose straight from a single tank, and on days when the ageing tank was skipped for cleaning. Say inflow rises in the rainy season and flocculant runs short, so an operator transfers freshly made solution to the day tank after half an hour. The solution looks clear, but a fingertip dipped in it feels less slimy and gritty with fine grains, and that afternoon the floc is smaller than usual.

Ageing is the time it takes for a solution that looks dissolved to become able to work. Just after dissolving begins, the polymer sits in agglomerates of many entangled chains, which come apart one by one over time, and it is these freed single chains that actually do the flocculating. In tests that varied ageing from one hour to six days, the required dose fell with ageing and was best at 72 hours, while a one-hour-old solution needed about 75% more (Owen et al., 2002). That study used nonionic products for mineral processing, and drinking water guidance calls for ageing with gentle mixing for 1 to 4 hours, checking product-specific times with the manufacturer (NHMRC, n.d.). With too little ageing, gel grains too small to see remain, and they behave like lumps in the flocculation tank or catch on strainers.

Ageing time comes straight from the records. For each batch, note the gap between the end of dissolving and the start of dosing, and compare it with the ageing time in the TDS. If there are separate make-down and ageing tanks, see whether the transfer point is kept, and check whether the setup draws from the same tank it is dissolving in. Jar tests with solution from one batch aged 30 minutes, 2 hours and a day put a number on the right ageing time for this site.

If ageing turns out to have been short, build in a structure that buys time between make-down and dosing. Split into two tanks, dosing from one while the other dissolves and ages, or with a single tank, interlock the transfer pump so it cannot run before the minimum ageing time has passed. Recalculate make-down tank capacity and batch frequency for high-demand seasons, and take the ageing time set by jar tests as the standard.

Hypothesis 4: hardness and chlorine

If the problem began after the make-up water changed, look at the water. That covers switching from mains water to groundwater or industrial water, reusing treated effluent for make-down, and using disinfected water. During works that cut the mains supply, flocculant is made down with groundwater for a few days; the solution looks thinner and cloudier than usual, and the same dose gives smaller floc. From the day mains water returns, the solution is clear again.

Hardness is the amount of divalent ions such as calcium and magnesium. These ions bind to negatively charged polymer chains more tightly than monovalent ions, making the chains contract, and they bridge chain to chain, lowering the viscosity of the solution. There are also reports that anionic polyacrylamide with a high degree of hydrolysis links up and precipitates when divalent ions are very plentiful (Akbari et al., 2017). Contracted chains bridge particles less well, since bridging relies on extended chains, and polymer that has linked up and settled out can show up as lumps. Chlorine harms the chains another way. Drinking water guidance notes that making up polymer solution with chlorinated water can reduce its effectiveness (NHMRC, n.d.), and in tests on polyacrylamides for potable water, one hour of chlorine exposure cut flocculation performance by about 20 to 35%, while the cationic product lost 25 to 35% after just five minutes of contact (Cheng, 2004).

The water can simply be measured. Measure total hardness, residual chlorine and pH of the make-up water, compare them with the make-up water conditions in the TDS, and set the date the water changed beside the date the trouble began. A control trial is the clearest test. Dissolve the same powder the same way in site make-up water and in softened or purified water, and compare lumps, viscosity and jar test performance. A large difference points to the water.

In that case, change the make-up water before the flocculant. Pass the make-down water alone through a softener, or bring in low-hardness water dedicated to make-down. If there is residual chlorine, run the water through an activated carbon filter or use chlorine-free water, and keep cationic products in particular away from chlorine. If the water cannot be changed, choose again with the supplier, by jar test, a product that loses less performance in that water.

Hypothesis 5: stored too long

Consider this hypothesis for solution made in quantity before a weekend or holiday, for day tanks that are only ever topped up and never emptied, and for outdoor tanks in the sun. A plant makes several times its usual volume before a long holiday and starts up again afterwards. The dose is the same, but floc will not form well, and stirring the tank bottom with a rod brings up stale gel lumps and scraps of film.

Dissolved polymer changes little by little over time. In tests on cationic polyacrylamides for papermaking, the ester bonds holding the cationic groups reacted with water and broke, so the positive charge fell, and this hydrolysis ran faster at higher pH and temperature. For one product, the cationic groups had a half-life of about 10 days even at 22 °C and pH 6 (Aksberg & Wågberg, 1989). Another study on cationic products of the same type also found hydrolysis speeding up with pH and temperature, and the hydrolysed polymer was less able to bridge particles, so the aggregates were smaller (Seo et al., 2018). Polyacrylamide is reviewed as also degrading through heat, light, chemical reactions, microbes and mechanical force (Caulfield et al., 2002). In tanks that are topped up and never emptied, gel left on the bottom and walls builds up, and stale gel mixed into new solution comes out as lumps.

Count the solution's age first. Check whether each batch has its date and time written on the tank, how many days it takes to use up, and when the tank was last emptied and cleaned, and compare that period with the solution storage life in the TDS. Jar-test a freshly made, aged solution from the same powder side by side with the stored solution, and the performance gap shows at once. Look at tank temperature, make-up water pH and whether sunlight reaches the tank as well.

If storage looks like the cause, match the amount made to the rate of use. Make batches small enough to be used within the TDS storage life, and before a holiday, rather than making extra, make the first batch after it early and let it age. Empty the tank completely at set intervals, wash the gel off the bottom and walls, then refill, and shade outdoor tanks from sun and heat. For cationic products with a short storage life, also review with the supplier whether to reset the make-down concentration within the TDS range.

Finding the cause

The five hypotheses take different effort to check. Ageing time and solution age need only the records, and the method of addition and mixing need only watching one batch being made. The make-up water takes a little time to test for hardness and residual chlorine, and control trials and jar tests come last. The steps before the control trials can be finished beside the tank within a day.

The look of the lumps points to the cause. Grains with a clear outside and a dry white core clumped at the moment of addition, so look at feed rate and dispersion. Gel pooled in the bottom corners suggests weak mixing, and solution that looks evenly dissolved but performs poorly after long high-speed mixing suggests cut chains. No visible lumps, but fine gel on the strainer and small floc, points to short ageing. Solution thinner or cloudier than usual points to the water, and performance that worsens with batch age points to storage.

If that does not settle it, run control trials in beakers. Dissolve the same powder at the same concentration, changing only one thing at a time. Set side by side solution fed through an eductor and solution dumped in at once, site water and softened water, 30-minute and one-day ageing, fresh and stored solution, and jar-test each on the same raw water. Strain the remaining gel through the same sieve and compare its weight or amount, and compare viscosity with the same viscometer or by timing flow through the same funnel.

Confirm the result in numbers. Check from the operating records that the lumps on the strainer have gone and that the dose needed for the same flocculation performance on the same raw water has come down. The job is done only when overflow turbidity and sludge condition have recovered with it.

Causes often overlap. Running high-speed mixing for a long time to break lumps from a dumped bag leaves the lumps and cuts the dissolved chains. A short-aged batch made down in hard water suffers two losses at once. In such cases, fix the method of addition and the make-up water first, then reset mixing and ageing time by jar test, and finally fit the storage period to the result, because while lumps keep forming, the effect of changing mixing or ageing cannot be compared fairly.

Limits and cautions

Suitable make-down concentration, mixing conditions, ageing time, storage life and make-up water conditions depend on the product's ionic type, molecular weight and form, so numeric decisions follow the flocculant's TDS and the supplier's guidance. Figures from studies come from their own products and conditions, so confirm them by jar test before applying them on site. Flocculants for drinking water treatment must meet use and residual limits, and those decisions follow confirmation from the authorities and the supplier.

Safety matters too. Handle powder so it does not become airborne, and wear a dust mask, goggles and gloves according to the product's safety data sheet, the SDS. Spilled powder or solution becomes very slippery when wet, so sweep it up dry before washing down. It is also known that degrading polyacrylamide can release acrylamide, a toxic monomer (Xiong et al., 2018), so dispose of old or spoiled product according to the SDS and local regulations.

Sources

  1. Akbari, S., Mahmood, S. M., Tan, I. M., Ghaedi, H., & Ling, O. L. (2017). Assessment of polyacrylamide based co-polymers enhanced by functional group modifications with regards to salinity and hardness. Polymers, 9(12), 647. https://doi.org/10.3390/polym9120647
  2. Aksberg, R., & Wågberg, L. (1989). Hydrolysis of cationic polyacrylamides. Journal of Applied Polymer Science, 38(2), 297–304. https://doi.org/10.1002/app.1989.070380211
  3. Caulfield, M. J., Qiao, G. G., & Solomon, D. H. (2002). Some aspects of the properties and degradation of polyacrylamides. Chemical Reviews, 102(9), 3067–3084. https://doi.org/10.1021/cr010439p
  4. Cheng, P. (2004). Chemical and photolytic degradation of polyacrylamides used in potable water treatment [Master's thesis, University of South Florida]. https://digitalcommons.usf.edu/etd/993
  5. Li, J., Zhou, W., Cai, C., Wang, S., & Zhu, J. (2023). Effect of agitation on the dissolution of APAM with different molecular weights and the equivalent diameter of coal slime settling floc with different particle sizes. Minerals, 13(2), 204. https://doi.org/10.3390/min13020204
  6. National Health and Medical Research Council [NHMRC]. (n.d.). Polyacrylamide. Australian drinking water guidelines, Part 5: Treatment chemicals. Retrieved November 2026. https://guidelines.nhmrc.gov.au/australian-drinking-water-guidelines/part-5/treatment-chemicals/polyacrylamide
  7. Owen, A. T., Fawell, P. D., Swift, J. D., & Farrow, J. B. (2002). The impact of polyacrylamide flocculant solution age on flocculation performance. International Journal of Mineral Processing, 67(1–4), 123–144. https://doi.org/10.1016/S0301-7516(02)00035-2
  8. Scott, J. P., Fawell, P. D., Ralph, D. E., & Farrow, J. B. (1996). The shear degradation of high-molecular-weight flocculant solutions. Journal of Applied Polymer Science, 62(12), 2097–2106.
  9. Seo, D., Oh, K., Im, W., & Lee, H. L. (2018). Hydrolysis of cationic polyacrylamide and its effect on flocculation of ground calcium carbonate. BioResources, 13(3), 5303–5318.
  10. Sojka, R. E., Lentz, R. D., Bjorneberg, D. L., & Aase, J. K. (1998). Station note 02-98: The PAMphlet. USDA-ARS Northwest Irrigation and Soils Research Laboratory. https://www.ars.usda.gov/pacific-west-area/kimberly-id/northwest-irrigation-and-soils-research/docs/station-notes/station-note-02-98-the-pamphlet/
  11. Xiong, B., Loss, R. D., Shields, D., Pawlik, T., Hochreiter, R., Zydney, A. L., & Kumar, M. (2018). Polyacrylamide degradation and its implications in environmental systems. npj Clean Water, 1, 17. https://doi.org/10.1038/s41545-018-0016-8

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.