Why does powder coating chip or peel on impact?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Coatings & Surface Treatments

Building the film thicker is the usual response when powder coating chips on impact, on the view that the powder is too weak, but an excessively thick film is itself prone to chipping, and impact resistance depends not only on thickness but heavily on the state of cure and the interface with the metal. What actually lies behind it can be under-cure, over-baking, a weak pretreatment coating, a film that is too thick or oil left on the metal, and sometimes two or more at once.

Background

A tool barely knocks a powder-coated part during packing or assembly, and at that spot the coating cracks in a star or flakes off in a coin-sized piece, leaving bare metal. After delivery, knocks in transport and dents from the customer's assembly line turn straight into appearance claims, and each flaked spot is where rust will start. When this keeps happening across a lot, parts may even have to be stripped for recoating.

On impact the metal dents in an instant, and the coating on it has to stretch and bend with it at the same instant. There are two ways the coating can fail. If the film cannot stretch that far, it cracks; if the bond between film and metal is weaker than the force of that moment, the film comes off whole. The standard impact test works the same way, dropping a weight to deform coating and substrate rapidly together and then examining the damage (ASTM International, 2024a).

A properly cured powder applied correctly over a clean, pretreated substrate should not suffer adhesion failure, and chipping of powder coatings is described as usually occurring between the coating and the substrate (Biller, 2021). So the causes divide into cure and thickness, which decide how far the film can stretch, and pretreatment and substrate cleanliness, which decide the bond at the interface.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: keep the flakes that came off and look at both faces, then compare the lot's oven, pretreatment and film thickness records with the cure schedule and recommended film thickness in the powder's TDS.

Hypothesis 1: under-cured

Cure tends to fall short when heavy castings or thick parts hang on the same rack as thin sheet metal and pass through the oven at the same speed, when the oven is not fully up to heat, as on a first run on a winter morning, and when conveyor speed has been raised for output. Powder cures only when the metal of the part, not the oven air, holds the set temperature for the set time. Say a line hangs thin covers and thick brackets on one rack. At outgoing inspection the covers survive impact while brackets on the same rack shed coating as if it crumbled.

In the oven the powder first melts and flows, then resin and curing agent react to build a network and harden. Differential scanning calorimetry, DSC, can separate this process into melting, flow, onset of cure and final cure (Mafi et al., 2005). A film whose reaction is unfinished has a loose network and does not reach its proper glass transition temperature, Tg, the temperature at which the hardened resin turns glassy and rigid; measuring the remaining reaction heat and the Tg by DSC shows how far the cure has gone (Belder et al., 2001). Such a loose film lacks the strength to stretch and hold under impact, and field troubleshooting guidance also notes that under-cured powder coatings are prone to chipping (Biller, 2021).

Start with a solvent rub test. A cloth soaked in solvent is rubbed back and forth over the film a set number of times to see whether coating dissolves onto the cloth or softens; a standard exists, so it can be repeated under the same conditions (ASTM International, 2024b). Solvent resistance differs by powder type, though, so the pass criterion follows the supplier's recommended conditions for that powder. Next, run an oven data logger through with the parts, attached to the thickest part, and check from the curve how many minutes the metal temperature met the cure schedule in the TDS. If the answer is still unclear, send a flake to a laboratory to measure Tg and remaining reaction heat by DSC.

If cure fell short, reset oven conditions on the basis of part metal temperature. Separate parts of very different thickness onto different racks, or set speed and temperature for the heavy parts, and do not send the first rack in before the oven has finished heating up. Repeat the data logger run at every change of season and every change of part mix, and do random solvent rubs on every lot. Sort parts already shipped by the same test, and agree with the supplier whether under-cured ones are re-baked or recoated.

Hypothesis 2: over-baked

Weigh up over-baking when parts sat in the oven for a long time while the line was stopped, when thin, light parts were baked on a schedule set for thick parts, and when parts already baked once went back into the oven for recoating. All the more so on lines where the temperature has been set generously out of worry about under-cure. Take a day when the conveyor stopped over lunch. Parts on the racks left inside the oven are slightly more yellow than the others and have lost gloss, and during assembly only those parts shed coating that flies off like chips of glass.

Heat completes the cure, but beyond what is needed it damages the film. Carbon-based raw materials such as resins and organic pigments break down at high temperatures, and a film baked too long or too hot loses gloss and changes colour or yellows. Resistance to over-baking varies with the powder type: epoxies are classed as poor because they yellow readily, while polyesters are classed as good (Diamond Vogel, n.d.). How coatings become brittle has been studied in detail in weathering research, which describes chain scission and changes in crosslinking as lowering how far the film can stretch while stress builds, so the film embrittles (Croll, 2022). Excessive heat can push the film in the same direction. The problem is sharper with recoats: chipping is reported at the boundary between coats when a second coat goes over a first coat that was over-baked (Biller, 2021).

Put colour and gloss side by side with parts baked under normal conditions. With a gloss meter and a colorimeter, compare them in numbers, and see whether chipping is concentrated on such parts. Find in the oven records when the line stopped and which racks were inside the oven then, and confirm from the data logger curve how far the metal temperature of light parts exceeded the cure schedule in the TDS. On recoated parts, check whether the first coat is still stuck to the back of the flake, that is, whether it came off between coats.

The remedy here is to set an upper limit on oven conditions. Check the cure range and over-bake limit in the TDS, build racks so that both light and heavy parts fall inside it, and set a procedure for pulling racks out of the oven or lowering oven temperature when the line stops. For recoating, follow the supplier's method and first confirm adhesion to the first coat in an inconspicuous spot.

Hypothesis 3: weak pretreatment

This hypothesis moves to the front when pretreatment concentration, temperature and pH have not been measured for a while, when rinse water has gone dirty, when iron phosphate meant for steel is used unchanged on aluminium, and right after phosphating has been replaced with a newer treatment such as zirconium. Mixed-metal parts are particularly difficult. Think of a plant that runs steel and aluminium parts alternately through the same pretreatment line. In the impact test the steel parts pass, while on aluminium parts the coating lifts widely around the point of impact, and the backs of the flakes are smooth.

A large part of how well powder coating holds to metal comes from the pretreatment coating. Phosphate conversion coatings, which build a crystalline layer on the metal, have long been used to raise paint adhesion and corrosion resistance (Narayanan, 2005), and zirconium or titanium conversion coatings do the same job with a far thinner oxide layer but are sensitive to bath pH and concentration and to the cleanliness left by the earlier stages (Milošev & Frankel, 2018). When the coating does not form properly, or does not suit the metal, the powder ends up bonded to a thin surface oxide or leftover contamination, and at the moment of impact it comes away along that weak boundary. Field troubleshooting guidance likewise points out that iron phosphate, which works well on steel, does not give the same adhesion on aluminium, and that steel composition varying from lot to lot can upset the pretreatment reaction (Biller, 2021).

The backs of the flakes and the exposed metal are the first clues. A smooth flake back and metal showing little of the colour or texture of a pretreatment coating point to the interface. Rate adhesion with the standard test that cuts a lattice through the film, applies and pulls off tape, and counts the squares lost (ISO, 2020). Check the records of bath concentration, temperature and pH and rinse water conductivity for that day against the supplier's control ranges, and split the failures by metal type and by steel lot to see whether they cluster.

Putting pretreatment right starts with holding the control ranges. Measure bath concentration, temperature and pH every shift and keep them within the supplier's ranges, and set a conductivity limit for rinse water, replacing it when exceeded. For mixed-metal parts, choose with the supplier a chemistry suited to those metals, and when switching to a new treatment, run impact and adhesion tests on each metal before production. If results split by steel lot, ask the steel supplier for composition and surface condition data.

Hypothesis 4: film too thick

Film easily exceeds the TDS range when gun output is raised to reach edges and corners, when a coated part is recoated because of a defect, and when automatic guns are set so their patterns overlap on large faces. This hypothesis weighs more after the film has been built up to stop chipping. At outgoing inspection there is a box that holds only recoated parts. Single-coated parts take an impact with only a small mark, while recoated parts crack in a ring at the same impact and shed large flakes.

The relation between thickness and stress is the key. As the film hardens and cools it tries to shrink, but being stuck to the substrate it cannot shrink freely, so a tensile stress remains in the plane of the film. At the same stress, a thicker film stores more energy, which is described as raising the drive to crack or to come away from the substrate (Francis et al., 2002). On top of that, when impact bends the substrate, the outer surface of a thick film must stretch further. Field troubleshooting guidance also lists excessively thick coatings as a cause of chipping and recommends keeping to the film thickness guidance in the TDS (Biller, 2021; Casebolt & Biller, 2025).

A film thickness gauge settles it quickly. Use a magnetic gauge on steel and an eddy current gauge on aluminium to measure the same spots on chipped and sound parts, following the standard's practice for number of readings and calibration (ASTM International, 2022). Note whether parts were recoated and which faces run thick. If chipping clusters on thick areas and recoated parts, the evidence points here.

Bringing film thickness back within the TDS comes first. Reset gun output, distance and overlap, and to cover edges, make a separate gun pass along them instead of building up the whole face. Recoat only by the supplier's approved method and within the total thickness it allows, and strip and recoat parts beyond that. Put thickness measurement at set spots on every lot into the inspection sheet.

Hypothesis 5: oil on the metal

Oil survives pretreatment on steel delivered with rolling or rust-preventive oil, on parts carrying press and machining fluids, from bare-hand prints, and when the degreasing bath is spent or has dropped in temperature. Watch for it all the more on material where the oil load can vary widely, such as hot-rolled steel that is pickled and oiled before delivery. Some lines let machined parts pile up for a day or two before pretreatment. Most are fine, but coating peels off in round patches only on the face that met the press die or around holes, and the exposed metal shines.

Oil slips a weak layer in between film and metal. Where oil remains, the pretreatment chemistry cannot reach the metal and no coating forms, and the powder that melts and flows over it sits on an oil film rather than on metal. Field guidance also notes that the oil on pre-oiled steel varies widely and changes how the cleaning stage performs, and that if the oil is not fully removed the following pretreatment will not work properly (Biller, 2021). In tests on liquid epoxy coatings rather than powder, engine oil or silicone oil on steel lowered adhesion strength, and on contaminated panels the coating mostly failed at the interface between coating and metal (Moshkriz et al., 2026).

Pour water on it. The water-break test, a standard method, takes parts after degreasing and rinsing and checks whether water spreads as an even film or breaks apart and beads where oil remains (ASTM International, 2021). See whether peeling clusters where oil readily collects, such as press faces, around holes and where hands touch, and check degreasing bath concentration and temperature records together with the incoming lot of the material.

Removing oil means matching the degreasing stage to the material. Keep degreaser concentration and temperature within range, and for heavily oiled material or parts carrying different machining fluids, reset the degreaser and process time with the supplier. Add the water-break test to the routine checks on the pretreatment line, and for parts that sit long after machining, wipe them before stacking or shorten the waiting time. Set a glove rule so that no one handles pretreated parts bare-handed.

Finding the cause

Rule out the five hypotheses starting with what samples in hand and existing records can show. Film thickness, solvent rubs and the water-break test take minutes on site, and oven and pretreatment records already exist. Data logger runs and DSC take more time and money, so they come next.

Where the flake parted is the biggest clue. Shiny bare metal and a smooth flake back point to the interface, so look first at pretreatment and oil, and give oil more weight if those spots cluster on press faces or around holes. If the film cracked and crumbled within itself, leaving a thin layer of coating on the substrate, the film could not stretch, so look at cure and thickness. Within that, softening under a solvent rub points to under-cure, clustering on yellowed parts that have lost gloss to over-baking, and clustering on recoated parts and thick areas to film thickness. If recoated parts part between coats, suspect over-baking of the first coat.

If that still does not settle it, make control panels. From the same material, make panels that differ in one thing only, such as longer degreasing, a different film thickness or a different oven time, and test them on the same day with the same impact tester. Numerical impact results reproduce poorly between laboratories, so use them for comparisons within one laboratory, where ranking is the safer comparison (ASTM International, 2024a).

The final check is made on production parts. After correcting the cause, run the same impact and cross-cut adhesion tests on every lot, and count chipping after the customer's assembly line and after transport on the same basis as before. The job is done only when those figures recover.

The hypotheses can overlap. Parts with oil left on them tend to carry a weak pretreatment coating as well, mixing parts of different thickness on one rack tends to leave some under-cured and others over-baked, and recoating brings thickness and over-baking together. In such cases, correct the interface first, because while degreasing and pretreatment are unsettled, the effect of changing the oven or the film thickness cannot be compared fairly.

Limits and cautions

Cure temperature and time, over-bake limits, recommended film thickness and pretreatment control ranges differ by powder and by pretreatment chemistry, so numeric decisions follow the product TDS and the supplier's guidance. Solvent rub results vary with the powder type, so they do not decide pass or fail on their own; use them to compare with sound parts in the same powder. For safety parts or parts under a separate customer specification, that specification's test methods and criteria take priority.

Safety matters too. Solvents used for rub tests are flammable, so keep ignition sources away and follow the SDS for gloves and ventilation. Pretreatment chemicals and degreasers are acids and alkalis, so wear eye protection and chemical-resistant gloves; use respiratory protection against powder dust, and keep dust from building up. For hot parts and work inside ovens, guard against burns and follow the entry procedure.

Sources

  1. ASTM International. (2021). ASTM F22-21, Standard test method for hydrophobic surface films by the water-break test. https://store.astm.org/f0022-21.html
  2. ASTM International. (2022). ASTM D7091-22, Standard practice for nondestructive measurement of dry film thickness of nonmagnetic coatings applied to ferrous metals and nonmagnetic, nonconductive coatings applied to non-ferrous metals. https://store.astm.org/d7091-22.html
  3. ASTM International. (2024a). ASTM D2794-93(2024), Standard test method for resistance of organic coatings to the effects of rapid deformation (impact). https://store.astm.org/d2794-93r24.html
  4. ASTM International. (2024b). ASTM D5402-19(2024), Standard practice for assessing the solvent resistance of organic coatings using solvent rubs. https://store.astm.org/d5402-19.html
  5. Belder, E. G., Rutten, H. J. J., & Perera, D. Y. (2001). Cure characterization of powder coatings. Progress in Organic Coatings, 42(3–4), 142–149. https://doi.org/10.1016/S0300-9440(01)00149-7
  6. Biller, K. (2021, September 22). Troubleshooting field defects. Powder Coated Tough. https://www.powdercoatedtough.com/News/ID/5256/Troubleshooting-Field-Defects
  7. Casebolt, E., & Biller, N. (2025). Beneath the surface: Understanding and preventing powder coating defects [Webinar slides]. The ChemQuest Group. https://chemquest.com/wp-content/uploads/2025/02/Understanding-and-Preventing-Powder-Coating-Defects-2025-webinar.pdf
  8. Croll, S. (2022). Stress and embrittlement in organic coatings during general weathering exposure: A review. Progress in Organic Coatings, 172, 107085. https://doi.org/10.1016/j.porgcoat.2022.107085
  9. Diamond Vogel. (n.d.). Technical brief #8: Overbake resistance of powder coatings. Retrieved November 2026. https://www.diamondvogel.com/sites/vogelindustrial.com/files/documents/TechBrief_8_OverbakeOfPowderCoatings.pdf
  10. Francis, L. F., McCormick, A. V., Vaessen, D. M., & Payne, J. A. (2002). Development and measurement of stress in polymer coatings. Journal of Materials Science, 37(22), 4717–4731. https://doi.org/10.1023/A:1020886802632
  11. International Organization for Standardization [ISO]. (2020). ISO 2409:2020, Paints and varnishes — Cross-cut test. https://www.iso.org/standard/76041.html
  12. Mafi, R., Mirabedini, S. M., Attar, M. M., & Moradian, S. (2005). Cure characterization of epoxy and polyester clear powder coatings using differential scanning calorimetry (DSC) and dynamic mechanical thermal analysis (DMTA). Progress in Organic Coatings, 54(3), 164–169. https://doi.org/10.1016/j.porgcoat.2005.06.006
  13. Milošev, I., & Frankel, G. S. (2018). Review—Conversion coatings based on zirconium and/or titanium. Journal of The Electrochemical Society, 165(3), C127–C144. https://doi.org/10.1149/2.0371803jes
  14. Moshkriz, A., Ekbrant, B. E. F., & Kiil, S. (2026). Adhesion investigation of waterborne and solventborne epoxy coatings on oil-contaminated and surface-corroded steel substrates. Progress in Organic Coatings, 221, 110534. https://doi.org/10.1016/j.porgcoat.2026.110534
  15. Narayanan, T. S. N. S. (2005). Surface pretreatment by phosphate conversion coatings – A review. Reviews on Advanced Materials Science, 9, 130–177. https://ipme.ru/e-journals/RAMS/no_2905/narayanan.html

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.