Turning up the voltage and holding the gun closer to spray again is the usual response when powder will not reach inside corners, but field lines crowd onto outer edges rather than into recesses, so spraying harder tends to thicken the outside while the inside stays bare. What actually lies behind it can be the Faraday cage effect, poor earthing, wrong voltage and current settings, a change in particle size, or gun distance and humidity out of range, and sometimes two or more at once.

Background

In the inner corners of box-shaped enclosures, the crevices of welded frames and the folded insides of brackets, too little powder sticks and bare metal shows through in patches. The operator aims the gun at the spot for a long time to add more, but meanwhile the outer faces and edges keep getting thicker, and the corner itself barely improves. More powder is used, more time goes in, and in the end the part may be touched up by hand or stripped and recoated.

Poorly covered recesses are not only a cosmetic problem. In a study that varied film thickness from 75 µm down to 25 µm to imitate the thin film in recesses, corrosion resistance measured by impedance fell by half as the film thinned, and panels whose powder layer had been put through back ionisation were lower still at the same thickness (De et al., 2002). Inner corners are also where water and dirt tend to collect, so a thin film there can be where rust starts first.

A corona gun applies high voltage to the electrode at its tip to ionise the air, and those ions attach to the powder and charge it. The charged powder flies to the earthed part under the combined pull of the airflow, the space charge of the powder cloud itself, gravity and the electric force between gun and part (Bailey, 1998). Because powder mainly travels along field lines, protruding areas and edges where field lines crowd are coated thickly, and recesses that field lines barely enter are coated thinly. So where powder lands is decided by the shape of the part, the earthing, the gun settings, the powder particles and the air between gun and part, all together.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: record the poorly covered spots with photos and film thickness, note the gun voltage and current, powder and air flow, hanger condition and booth temperature and humidity at the time, and compare them with the powder's technical data sheet, the TDS, and the conditions in the equipment manual.

Hypothesis 1: Faraday cage effect

Start with this hypothesis when the shape of the part is itself recessed: grooves deeper than they are wide, inside corners where three faces of a box meet, weld crevices, and the gaps between closely spaced fins or wire mesh. A typical case is a new part of a different shape whose insides stay bare though no setting has changed. Say an operator is coating the inner corner of an electrical enclosure. With the gun aimed straight at the corner, the powder cloud spreads out at the opening and builds up only along the edges of the two walls, while deep in the corner the metal stays bare.

The Faraday cage effect arises because the electric field cannot get far into a recess. A strong field forms between the corona gun tip and the earthed part, and another forms between the net-charged powder cloud and the part. Powder builds up thickly where field lines crowd while recesses are left uncoated, and this happens with both corona and tribo charging as long as the powder cloud carries a net charge (Biris et al., 2005). A study that calculated the field over a plate with a cavity found that the deeper and narrower the cavity, the weaker the field inside it, and that the field was strong at the corners (Osman et al., 2014). So powder sticks first to the edges of the opening, thickening them, and gets no force to carry it further in.

Measure the recess first. Note the width of the opening and the depth, then measure and compare dry film thickness on the inside floor and walls, at the edges of the opening and on the outer face (ASTM International, 2022). Where a probe will not fit, cut a sample of the same shape and look at the cross-section, or photograph how the powder has settled after spraying and before curing. A pattern that is thick at the edges of the opening and thinner further in points to this hypothesis.

When shape is the cause, change the order and the aim. Coat the inside first and the outer faces afterwards. Overspray from the inside also lands on the outer faces, so coating the outside first and then going back into the recess tends to thicken only the outside further. Aim along one inner wall rather than at the opening, and use a long or angled nozzle made for recesses if one is available. Tribo guns have been proposed to cover recesses better because they produce powder charged both positively and negatively without free ions (Biris et al., 2005), so if such parts are common, a trial with the equipment supplier is worth running.

Hypothesis 2: poor earthing

Look at earthing first when the whole part, not just the inside, is coated thinly and such parts cluster on certain hangers or a certain stretch of conveyor. It happens when cured coating has built up layer on layer on hangers and hooks, when hanger stripping has been put off, when a part hangs only by a coated face or the edge of a hole, and when conveyor rails and earth leads are dirty or loose. Hangers that have not been stripped for weeks go back on the line. Every hook is thick with coating, and parts on those hangers are thinner than usual even on the front face, with the inner corners nearly bare.

The field that draws charged powder in forms only when the part is earthed. When the earth path breaks or its resistance rises, charge from the powder landing on the part cannot drain away; the part charges up to the same polarity as the powder and repels what comes next, so even the front face takes less. Recesses, where the field was weak to begin with, lose what little they had and go bare first. Charge collected on an unearthed part can also ignite the powder cloud with a spark, so the US Occupational Safety and Health Administration requires that all conductive objects in the spray area be adequately earthed, that objects being coated be kept in metal-to-metal contact with an earthed conveyor or support, and that hooks be cleaned regularly to keep that contact (OSHA, n.d.).

One resistance meter settles it. Measure the resistance between part and building earth on several hangers, and record clean hangers and coated-up hangers side by side. Use the limit set by the equipment supplier or the plant's safety standard as the reference. Hang identical parts on a freshly stripped hanger and an old one, spray them at the same settings, and compare film thickness on the front face and inside; that puts a number on how much earthing accounts for.

If any hanger reads high, rebuild hanger care. Set the stripping interval for hangers and hooks by output, and change the contact points where parts hang to sharp tips or knife edges that collect less coating. Add conveyor rails and earth leads to the routine inspection sheet, and record resistance readings whenever hangers are put back into service and at fixed intervals.

Hypothesis 3: wrong gun settings

Gun settings are where people often reach when chasing film thickness. The cases in point are when the voltage is left at maximum while the gun passes the same spot again and again to build thickness, when the current limit has been switched off, or when automatic gun settings made for another product are used as they are. The day after a complaint about low thickness, an operator turns the voltage all the way up and goes back and forth over the same area. Small crater-like marks and a rough texture appear on the outer face, while the inner corner is still bare.

Of the ions a corona gun produces, only about 6 to 10% go into charging the powder; most of the remaining free ions settle on the powder layer and the part, building up charge in the layer and bringing on back ionisation sooner. In the same study, the appearance of the cured film varied with gun voltage (Biris et al., 2003). Back ionisation is discharge within the deposited powder layer when the field inside it grows too strong, and it leaves pinholes and craters in the film (De et al., 2002). Raising the voltage increases the charge on the powder, but back ionisation also intensifies as the layer grows, and the highest deposition efficiency came somewhere in between, where the two effects balance (Meng et al., 2008). A higher voltage strengthens the whole field between gun and part, so the pull towards outer edges can grow too, and the inside becomes that much harder to cover.

The numbers are on the gun display. Record voltage and current during spraying for each part, and check whether the current limit is on. Craters, pinholes and a rough texture on the outer face are clues that point to back ionisation. Spray identical parts at two or three voltage steps and set inner film thickness beside outer surface condition, and the point where a setting starts doing more harm than good shows itself.

If the settings look wrong, split them by area of the part. When coating the inside, lower the voltage and switch on the current limit to cut free ions and back ionisation; coat the outer faces at the standard setting; and store both settings for each product so the operator does not set them from scratch every time. Fitting an earthed ring electrode near the gun tip to collect free ions has been reported to reduce back ionisation at the cost of lower first-pass transfer efficiency (Biris et al., 2003), so weigh the trade-off with the equipment supplier before choosing it.

Hypothesis 4: changed particle size

Suspect the powder itself on lines that mix in a lot of reclaim, right after a switch to a fine thin-film powder, when a new powder batch has a different particle size, and when the sieve or separator in the reclaim system is worn. On a line that returns even the filter fines from the reclaim system to the hopper, the powder flow at the gun tip pulses and breaks up as the afternoon goes on, and the inner corners look emptier than in the morning.

Powder flows, charges and deposits differently depending on size. Powder that came back after one pass of electrostatic spraying had become finer, and fine powders under 30 µm flowed much worse after spraying (Fu et al., 2011). In a study comparing powders of similar median size, the share of very fine particles mainly governed flow and deposition efficiency, while the share of coarse particles governed film thickness uniformity and appearance (Zhu et al., 2024). Ultrafine powder lost deposition rate faster than coarse powder as spraying went on, and raising the voltage lowered the charge in its deposited layer, the opposite of the trend for coarse powder (Meng et al., 2009). Powder that flows unevenly leaves the gun in bursts, and powder whose deposition drops off quickly does not build up inside even when sprayed again.

Taking samples from the hopper and from a fresh box and comparing their particle size distributions is the first step. Log the reclaim ratio every shift, and watch whether the surface of the fluidised hopper boils evenly or shows channels and floating lumps. Spray identical parts once with fresh powder only and once with the usual hopper contents, compare inner film thickness and powder use, and the size effect becomes clear.

If the fines have grown, re-route the reclaim. Blend fresh powder and reclaim at a set ratio, do not return the very fine filter fraction to the hopper, and inspect sieves and separators regularly. Reset fluidising air pressure and gun conveying air so the powder flows evenly, and agree a particle size range with the supplier as a purchase specification, with a certificate for every batch.

Hypothesis 5: distance and humidity

When the same part at the same settings gives different results from person to person or season to season, look at the gun-to-part distance and the booth air. It happens when each operator holds the gun at a different distance, when automatic guns are not repositioned for the part size, when booth exhaust has been turned up, and when humidity swings, as in winter air dried out by heating or in the rainy season. In midwinter with the heating on full, parts sprayed with the same program as in autumn can show more small craters on the outer face and emptier inner corners.

Powder does not fly by electric force alone; it rides the airflow. A numerical model that included turbulent airflow in the booth and the space charge of free ions has been validated against experimental data (Shah et al., 2007), and powder deposited on the part lay in a cone-shaped pattern in front of the gun and built up more towards the edges of the panel (Meng et al., 2008). With the gun too close, powder and free ions crowd onto a small area and the layer there fills up quickly; too far, and the powder follows the airflow rather than the field and drifts past the part. Humidity changes the electrical resistance of the powder. When fine powder particles were made to take up moisture on their surfaces, resistivity fell, the field inside the deposited layer dropped, more charged powder could deposit, and first-pass transfer efficiency rose by up to 17% (Fu et al., 2013). Conversely, very dry air can be read as making the field in the layer build up quickly, so less powder can deposit.

Measure distance with a tape and the air with a logger. Measure each operator's distance from gun tip to part, and record automatic gun positions for each part size. Put a temperature and humidity logger in the booth and match its readings to the days with rejects, noting exhaust damper position and gun conveying air as well. Spray identical parts at two or three set distances and compare inner thickness, and the right distance for that part emerges.

If distance and air have been unsteady, put controls in place to narrow the range. Set a gun distance for each part in the work standard, and use positioning jigs or stored position values for automatic guns. Condition booth humidity to the range recommended by the powder and equipment suppliers, and check the humidity log daily in winter and the rainy season. Set exhaust at the level that keeps powder from escaping the booth, and do not change it at will.

Finding the cause

Earthing is the fastest to rule out. Measuring resistance takes minutes, and if earthing is bad, the effect of fixing anything else is hidden. Next come the values that can be read on the spot, such as voltage and current on the gun display, gun distance and booth temperature and humidity, and anything that needs samples sent out, such as particle size analysis, goes last.

The shape of the poorly covered area is the next clue. Thick at the edges of the opening and thinner further in puts the Faraday cage effect from the part's shape at the centre; evenly thin on the front face as well as inside sends you back to earthing. Craters or pinholes on the outer face as well point to free ions and back ionisation, which means voltage, current and gun distance. A problem that worsens over time with pulsing powder flow points to particle size and reclaim, and one that splits by season or operator points to gun distance and humidity.

When the clues point to more than one cause, separate them with control trials. Make pairs that differ in one thing only, such as a freshly stripped hanger against an old one, low voltage against high, fresh powder against hopper powder, or a near distance against a far one, spray identical parts, and measure film thickness at fixed spots inside. Change two conditions at once and there is no telling which one made the difference.

The final check is made under production conditions. Run for several days on the new settings and controls, and count inner film thickness at the fixed spots, powder use and the number of parts touched up, on the same basis as before the change. The job is done only when inner thickness stays above the TDS minimum and touch-ups have fallen.

Causes can also tangle. Raising the voltage to cover a recessed part adds free ions and brings back ionisation on sooner, and on a poorly earthed hanger the effect is greater. When reclaim adds fines, deposition efficiency drops and the operator falls back on voltage and extra passes again. In such cases, first correct earthing and the condition of the powder to fix the baseline, then reset voltage, current and distance to suit the shape of the part, because while the baseline is unsettled, the effect of a settings change cannot be compared fairly.

Limits and cautions

Suitable voltage, current, powder flow, gun distance and booth humidity differ with the type of gun and powder and the shape of the part, so numeric decisions follow the powder's TDS and the equipment supplier's manual. For parts whose recesses are so deep and narrow that no setting covers them, consider changing the shape at the design stage or combining another coating method, and take earth resistance limits from the plant's safety standard and the equipment supplier.

Safety matters too. Airborne powder can ignite from a flame or a static discharge, so earth every conductive object in the spray area, people included, and use the gun with its handle earthed (OSHA, n.d.). Handle powder with a mask and protective equipment as the product's safety data sheet, the SDS, directs, and switch off the high-voltage supply and discharge any remaining charge before cleaning the gun nozzle or touching the electrode.

Sources

  1. ASTM International. (2022). ASTM D7091-22, Standard practice for nondestructive measurement of dry film thickness of nonmagnetic coatings applied to ferrous metals and nonmagnetic, nonconductive coatings applied to non-ferrous metals. https://store.astm.org/d7091-22.html
  2. Bailey, A. G. (1998). The science and technology of electrostatic powder spraying, transport and coating. Journal of Electrostatics, 45(2), 85–120. https://doi.org/10.1016/S0304-3886(98)00049-7
  3. Biris, A. S., Mazumder, M. K., Sims, R. A., Yurteri, C. U., Farmer, S., & Snodgrass, J. (2003). The effect of ring electrodes attachment to a corona gun on control of free ion concentration and back corona for improving powder paint appearance. IEEE Transactions on Industry Applications, 39(6), 1614–1621. https://doi.org/10.1109/TIA.2003.819439
  4. Biris, A. S., Trigwell, S., Sims, R. A., & Mazumder, M. K. (2005). Study of velocity and materials on tribocharging of polymer powders for powder coating applications. NASA Technical Reports Server. https://ntrs.nasa.gov/citations/20120001362
  5. De, S., Biris, A. S., Mazumder, M. K., Yurteri, C. U., & Sims, R. A. (2002). Surface defects and corrosion in electrostatically deposited powder films. In Conference Record of the 2002 IEEE Industry Applications Conference, 37th IAS Annual Meeting (Vol. 4, pp. 2460–2465). https://doi.org/10.1109/IAS.2002.1042791
  6. Fu, J., Krantz, M., Zhang, H., Zhu, J., Kuo, H., Wang, Y. M., & Lis, K. (2011). Investigation of the recyclability of powder coatings. Powder Technology, 211(1), 38–45. https://doi.org/10.1016/j.powtec.2011.03.016
  7. Fu, J., Zhang, H., & Zhu, J. (2013). Improvement on the first pass transfer efficiency of fine polymer coating powders for corona spraying process. Advanced Powder Technology, 24(6), 1054–1062. https://doi.org/10.1016/j.apt.2013.03.007
  8. Meng, X., Zhang, H., & Zhu, J. (2008). The characteristics of particle charging and deposition during powder coating processes with coarse powder. Journal of Physics D: Applied Physics, 41(19), 195207. https://doi.org/10.1088/0022-3727/41/19/195207
  9. Meng, X., Zhu, J., & Zhang, H. (2009). The characteristics of particle charging and deposition during powder coating processes with ultrafine powder. Journal of Physics D: Applied Physics, 42(6), 065201. https://doi.org/10.1088/0022-3727/42/6/065201
  10. Occupational Safety and Health Administration [OSHA]. (n.d.). 29 CFR 1910.107, Spray finishing using flammable and combustible materials. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/laws-regs/regulations/standardnumber/1910/1910.107
  11. Osman, H., Adamiak, K., & Castle, G. S. P. (2014). Numerical simulation of the electric field distribution for electrostatic powder coating of targets with surface perturbations. In Proceedings of the ESA Annual Meeting on Electrostatics 2014. https://electrostatics.org/wp-content/uploads/2023/08/2014_H2_Osman.pdf
  12. Shah, U., Zhang, C., Zhu, J., Wang, F., & Martinuzzi, R. (2007). Validation of a numerical model for the simulation of an electrostatic powder coating process. International Journal of Multiphase Flow, 33(5), 557–573. https://doi.org/10.1016/j.ijmultiphaseflow.2006.12.001
  13. Zhu, X., Xie, J., Zhang, H., Liu, W., Zhang, H., & Zhu, J. (2024). Insights into powder coating excellence: Unveiling the effects of particle-size distribution. Progress in Organic Coatings, 197, 108815. https://doi.org/10.1016/j.porgcoat.2024.108815

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.