Replacing the impeller or filling worn areas with a repair compound is the usual response when a pump loses efficiency, but if whatever cut the metal is still there, the new surface tends to wear away in the same place. What actually lies behind it can be abrasion by sand and slurry particles, cavitation, erosion-corrosion where corrosion and wear act together, flow away from the operating point, poor surface preparation before a repair coating, or a coating whose type and thickness do not suit the wear, and sometimes two or more at once.

Background

The valve is open as far as it always was, yet the flowmeter reads lower and the tank takes a little longer to fill each time. Open the pump at the next overhaul and the impeller vane tips have thinned, while the casing has pitted in places or worn smooth. Moving the same volume now takes more power, meeting output means running the pump longer or bringing in the standby, and if performance suddenly collapses the line stops.

A pump's efficiency is set by the shape of the passages the liquid travels through and by the gaps between parts. Wear rings between impeller and casing form a narrow gap that separates the high-pressure side from the low-pressure side, and when particles, or liquid squeezing through the gap, open it up, liquid slips back from the high-pressure side to the suction side and efficiency falls. A cut or pitted impeller also loses performance and efficiency, and if material is lost unevenly the impeller goes out of balance, putting alternating loads on the bearings and raising vibration (DOE, 2006).

Flow inside a pump damages material in three main ways: abrasion by solid particles carried in the liquid, cavitation, where collapsing bubbles strike the surface, and erosion-corrosion, where corrosion and wear feed each other (Gülich, 2020). On top of these come operating conditions that intensify them, and repair coatings over worn areas that fail to do their job.

In such cases the technical team sets up the six hypotheses below and rules them out one by one. The start is always the same: keep the worn parts, photograph where and how they wore, and compare the flow, suction and discharge pressures, liquid temperature and solids content at the time with the pump curve and the specification sheet.

Hypothesis 1: abrasive solids

If the liquid carries hard solids such as sand, mineral fines, catalyst dust or sludge, start with this hypothesis. Intake pumps drawing river or ground water, pumps moving sludge from the bottom of a settling tank and pumps circulating washing liquid laden with grinding debris are typical, and solids can rise suddenly after heavy rain or once a suction strainer tears. Picture the overhaul of a settling-tank sludge pump. With the casing open, the tongue, the edge where the volute splits off towards the discharge, has been blunted, the gap between wear ring and impeller has visibly widened, and the leading edges of the vanes have worn round.

When hard particles carried by the flow strike a metal surface, those arriving at a shallow angle scratch and cut it, while those arriving head-on press dents into it. Ductile metals lose more to glancing impacts, hard but brittle materials suffer more from head-on ones, and the amount removed rises steeply with particle velocity (Finnie, 1960). Inside a pump, the angle and force of impact differ from place to place, so parts wear unevenly. In a test with specimens fixed along the casing wall of a slurry pump, wear at the tongue came from both cutting and deformation, while elsewhere material was removed by cutting and ploughing (Tarodiya & Gandhi, 2019). Solids lower head and efficiency compared with pumping water alone, and wear varies with particle size, concentration and operating conditions (Tarodiya & Gandhi, 2017).

The first thing to measure on site is the solids in the liquid. Draw a sample at the suction, weigh the solids in a set volume, sieve it to see particle size, and rub it between the fingertips to feel for grit. Particle size, hardness and the volume fraction of solids are criteria for selecting a pump, so compare the present values with the conditions the pump was chosen for (DOE, 2006). At strip-down, measure the wear-ring clearance against the manufacturer's manual and record where the wear is concentrated with photographs and thickness readings.

Once particles look responsible, cut them down before they reach the pump. Inspect strainers, settling tanks and separators such as cyclones, and confirm that the suction inlet sits high enough not to draw in sediment from the bottom. Reset widened wear-ring clearances to the manufacturer's manual or replace the rings. Because particle velocity strongly governs how much is cut away, check that the pump is not running faster than it needs to. Where the process cannot shed its solids, move on to matching materials or linings to the wear, a choice made together with coating type and thickness.

Hypothesis 2: cavitation

Cavitation goes hand in hand with conditions that lower the suction pressure: a low level in the suction tank, a clogged strainer in the suction line, hot liquid, or a pump running far beyond its design flow. On a summer afternoon, a transfer pump is drawing from a hot-water tank whose level is close to the bottom. A sound like gravel rolling comes from the pump, the pressure gauge needle trembles, and when the impeller is later opened its vanes show patches roughened like a sponge by clusters of small pits.

Cavitation is the formation of vapour bubbles in a liquid when its static pressure falls below the vapour pressure at that temperature. The bubbles are carried to where pressure rises again and collapse violently, sending high-velocity jets into nearby surfaces, and when that force exceeds the strength of the material, it is lost bit by bit. The vapour also obstructs the flow and lowers the head, and an eroded impeller goes out of balance, adding to bearing wear and vibration (DOE, 2006). Damage forms on surfaces close to where the bubbles collapse, and it is costly and very hard to eliminate (Brennen, 2011). It can occur not only at the vane inlet but also at the outlet and in diffusers (Gülich, 2020).

Begin with the suction gauge and the liquid temperature. From suction pressure, the vapour pressure at that temperature and the losses in the suction line, work out the net positive suction head available, the NPSHA, which is the pressure margin left at the pump inlet, and compare it with the NPSHR the pump requires at the actual flow. A common rule in system design is to keep NPSHA 25% above NPSHR at every expected flow (DOE, 2006). Recommended margins by application are set out in a Hydraulic Institute guideline, which explains that insufficient margin leads to noise, vibration, loss of performance and reduced reliability (HI, 2024). To compare materials for cavitation resistance, use the standard test in which a vibrating apparatus produces cavitation damage on a specimen face (ASTM International, 2021b).

If the margin comes up short, restore suction pressure. Raise the minimum operating level in the tank, clean the clogged strainer, cut needless bends and valve losses in the suction line, and see whether the liquid can be cooled. If the flow sits far above the design point, deal with that cause together with the operating point. Where some cavitation cannot be avoided, specify impellers in high-tensile-strength material (DOE, 2006).

Hypothesis 3: erosion-corrosion

Pumps handling seawater, chloride-rich cooling water or acidic or alkaline process liquid sometimes wear out quickly only in their fast-flow areas. When a material that rusts in that liquid, such as cast iron or carbon steel, also meets some solids or high velocity, check whether corrosion and wear are acting together. Open such a seawater cooling pump and the fast-flow vane tips and casing surfaces are gouged smooth to bright metal with no rust at all, while thick rust sits in the slow corners.

With corrosion alone, a thin film such as an oxide or a passive layer forms on the metal and slows further attack. But when fast flow, particles or collapsing bubbles strip that film away, bare metal is exposed and corrodes quickly, and the corroded, weakened surface is in turn cut away more easily (Wood, 2006). So the loss when both act together can exceed the sum of corrosion alone and wear alone, and a standard guide calculates that extra share separately as synergism. The same guide explains that reducing either wear or corrosion can lower the total loss (ASTM International, 2021a). A review of the past decade of research covers erosion-corrosion testing of materials including stainless steels, together with ways of protecting against the loss (Burson-Thomas & Wood, 2017).

Measure the liquid first. Check pH, chloride, dissolved oxygen, temperature and solids, and see whether they match the conditions the pump material was chosen for. On the stripped parts, set the fast-flow and slow-flow surfaces side by side and look at whether bare metal free of rust and deposits is confined to the fast-flow areas. If the shares need to be put in numbers, a laboratory measures weight loss under corrosion alone, wear alone and both together, and calculates the synergism (ASTM International, 2021a).

With the cause narrowed to erosion-corrosion, tackle whichever share is easier to reduce. Filtering out solids or lowering velocity cuts the mechanical share, while controlling pH and oxygen through water treatment or dosing a corrosion inhibitor cuts the corrosion share. If loss persists, change to an alloy that forms a robust protective film in that liquid, or consider surface treatments evaluated under erosion-corrosion, such as high-velocity oxy-fuel, or HVOF, sprayed coatings (Wood, 2006).

Hypothesis 4: off-BEP running

Operating-point trouble shows up on lines where a pump larger than the duty needs runs with its discharge valve heavily throttled, or where a process change has moved the flow well away from the design. Stopping one of two pumps running in parallel, or changing the piping so that system resistance shifts, can also push a pump far from its design point. Consider a line fitted early with a large pump in anticipation of expansion. It now runs with the discharge valve about half closed, bearings and mechanical seals have been changed several times over the years, and pits have appeared on the vane surfaces at the impeller suction.

Every centrifugal pump has a best efficiency point, the BEP, where efficiency is highest and radial bearing load is lowest. At the BEP, liquid enters the vanes and casing without shock and flows evenly, free of separation. Running far from the BEP can accelerate wear of bearings, mechanical seals and other parts. At too low a flow, internal recirculation sets in, with liquid swirling at the impeller suction or around its outer edge, and this flow causes damage much like cavitation. Running well beyond the design flow instead shrinks the gap between NPSHA and NPSHR dangerously, and a pump that manages with a small margin near the BEP needs a much larger one to suppress all cavitation away from it (DOE, 2006).

The operating point can be plotted on the curve with a few instruments. Take the flow from the line flowmeter or a clamp-on ultrasonic meter and the head from suction and discharge pressures, place the point on the pump curve, and see how far it lies from the BEP and from the manufacturer's minimum flow. Valve position and motor current records show when a process change moved the operating point. If the stripped impeller has cavitation-like damage at the suction or outer edge although suction pressure had margin, low flow becomes the stronger suspect.

If the operating point is far from the BEP, match the pump to the real duty. For a pump that is always heavily throttled, consider trimming the impeller to a smaller diameter, fitting a variable speed drive, or replacing it with a correctly sized pump. A process with widely swinging flow can split the duty across several pumps so that each stays near its BEP (DOE, 2006). If the flow ever drops below the minimum, keep the minimum flow with a bypass line.

Hypothesis 5: poor surface prep

When worn casings and impellers were rebuilt with a repair compound such as ceramic-filled epoxy and it came off in sheets within months, suspect the surface beneath before the coating itself. This can happen when a short shutdown meant grinding or wire-brushing instead of abrasive blasting, when cast iron that had pumped salty water for years was coated without washing, or when the compound went onto a surface wet with condensation on a humid day. At the next overhaul, open up a pump whose rust was simply ground off before the compound went on during a brief scheduled outage. The coating edges have lifted and torn away in the direction of flow, and rust has spread across the metal where it came off.

A coating protects only while it stays bonded to the metal, and the bond depends on how clean and how rough the surface is. On a surface still carrying rust, mill scale, oil or old paint, the coating bonds to that residue instead of the metal. That is why an international standard grades the cleanliness of blast-cleaned steel against photographic references (ISO, 2007), and a separate one specifies the comparator plates against which the roughness produced by blasting is judged (ISO, 2012b). Some contamination cannot be seen. Soluble salts such as chlorides and sulphates left between metal and coating draw in water that permeates the film, causing blisters and driving corrosion under the film, so the coating fails early (Morcillo, 1999).

Turn over a piece of the detached coating first. If its back carries rust or old paint and the metal beneath is bare, the coating never bonded properly to the surface; if it split within its own layer, look at the material and its cure instead. Check whether the repair records hold the blast grade and roughness readings, and whether surface temperature and dew point were measured before application, and test surface salts on any bare metal not yet coated.

When recoating, blast to the surface grade and roughness set in the coating maker's technical data sheet, the TDS, and record the result against the standard references. Wash surfaces that showed salts with clean water and coat only once a retest falls within the TDS limit. Coat blasted surfaces within the time the TDS allows, before rust returns, and start only after confirming that surface temperature is safely above the dew point.

Hypothesis 6: wrong coating

When the surface was properly prepared yet the coating has worn evenly through to the substrate or torn away, check whether it suits the wear at that spot. Typical cases are one repair material used on every pump, a coating meant for fine particles moved to a pump that also sees coarse ones, and thin application on vane tips and edges where building thickness is hard. Imagine a plant that put the same rubber-based coating on two pumps. On the pump moving water with fine sand it was nearly intact at the next overhaul, while on the pump that takes in coarse gravel it had torn and come away in places within weeks.

Each material wears in its own way, so no single material resists every condition. Ductile metals are more vulnerable to glancing impact, hard but brittle materials to head-on impact (Finnie, 1960). Elastomers wear less by cutting than metals do; under repeated impact, small cracks at the surface grow until material comes away (Arnold & Hutchings, 1990). In slurry-jet tests on pump lining materials, elastomer linings did not wear when particles were below a certain size while stainless steel under the same conditions did, and that critical size was 208, 91 and 42 µm for a fluid elastomer, rubber and polyurethane respectively (Iwai & Nambu, 1997). In other words, the same coating can hold up against fine particles yet fail against coarse ones.

The shape of the worn coating is the clue. Even thinning down to the substrate points to thickness or wear rate, while tears or chunks torn out suggest that particle size and impact angle do not suit that coating. Measure the remaining thickness with a magnetic or eddy-current gauge, following the standard method and acceptance criteria for rough, blast-cleaned surfaces (ISO, 2012a), and compare the readings with the thickness recommended in the TDS. For particle size and quantity, use the values measured when checking for abrasive solids.

If the coating did not suit the conditions, choose materials zone by zone according to how each wears. Elastomers may suit areas swept by fine particles and harder materials may do better where coarse particles strike hard, so give the coating supplier the actual particle size and impact conditions and ask for test data under them. On vane tips and edges, where coatings tend to run thin, build up to the TDS thickness in several coats, then measure and record the thickness.

Finding the cause

Six hypotheses still leave much that can be settled before the pump is opened. Operating point and suction conditions can be read straight off pressure gauges, flowmeters and thermometers, and the liquid's solids and chemistry can be measured from a single sample bottle. Strip-down and laboratory analysis come after that.

The shape of the damage is the next clue. Marks of particles cutting and ploughing together with widened wear-ring clearance point to solids in the liquid, and clustered pitting that coincides with records of low suction pressure points to cavitation. Bare-metal gouging confined to fast-flow areas, with rust in the slow ones, suggests erosion-corrosion, and damage at the impeller suction or outer edge despite ample suction pressure points to internal recirculation at low flow. A repair coating that came off in sheets with rust on its back points to surface preparation, and one worn evenly to the substrate or torn points to coating type and thickness.

If that still does not settle it, run control trials that change one thing at a time. Run with a higher suction tank level, move the operating point towards the BEP by changing the valve setting, and fit a new strainer to cut the solids. Change only one thing at a time, or there is no telling which one worked. To compare wear rates directly, small metal specimens fixed along the casing wall and weighed after a set running time have been used in testing, and placing them at several locations also shows where wear is fastest (Tarodiya & Gandhi, 2019).

After the repair, measure flow, head and power again and compare them with the pump curve and with the readings from before. If wear rings and impeller were replaced, the first verdict is whether performance has come back; the final one is whether the same spots, measured again at the next overhaul, are wearing more slowly.

The hypotheses can overlap. Collapsing bubbles and particles strip the film that held corrosion back and so intensify erosion-corrosion (Wood, 2006), running away from the BEP erodes the cavitation margin, and a coating on a poorly prepared surface fails early even if the material suits the duty. In such cases, put the operating point, suction conditions and solids right first, then choose materials and coatings, because while the forces doing the cutting are unchanged, changing only the coating gives no fair comparison between materials.

Limits and cautions

Suitable operating range, NPSH margin, wear-ring clearance, and coating surface grade and thickness differ by pump model, liquid and coating product, so numeric decisions follow the pump manufacturer's manual and the coating TDS. A cracked casing, or a wall thinned close to its design thickness, is not a job for a repair coating; leave the decision to the pump manufacturer or a pressure equipment specialist, and put material changes on pumps handling toxic or flammable liquids through the same process.

Before strip-down, isolate the pump both electrically and on the piping, and confirm it has been drained and depressurised. For process liquids, blasting dust, epoxies and solvents, follow each product's safety data sheet, the SDS, for protective equipment and ventilation, and when applying solvent-borne coatings in tight spaces such as inside a casing, manage ventilation and ignition sources together.

Sources

  1. Arnold, J. C., & Hutchings, I. M. (1990). The mechanisms of erosion of unfilled elastomers by solid particle impact. Wear, 138(1–2), 33–46. https://doi.org/10.1016/0043-1648(90)90166-8
  2. ASTM International. (2021a). ASTM G119-09(2021), Standard guide for determining synergism between wear and corrosion. https://store.astm.org/g0119-09r21.html
  3. ASTM International. (2021b). ASTM G32-16(2021)e1, Standard test method for cavitation erosion using vibratory apparatus. https://store.astm.org/g0032-16r21e01.html
  4. Brennen, C. E. (2011). Hydrodynamics of pumps. Cambridge University Press. https://doi.org/10.1017/CBO9780511976728
  5. Burson-Thomas, C. B., & Wood, R. J. K. (2017). Developments in erosion–corrosion over the past 10 years. Journal of Bio- and Tribo-Corrosion, 3(2), 14. https://doi.org/10.1007/s40735-017-0073-4
  6. Finnie, I. (1960). Erosion of surfaces by solid particles. Wear, 3(2), 87–103. https://doi.org/10.1016/0043-1648(60)90055-7
  7. Gülich, J. F. (2020). Centrifugal pumps (4th ed.). Springer. https://doi.org/10.1007/978-3-030-14788-4
  8. Hydraulic Institute [HI]. (2024). ANSI/HI 9.6.1-2024, Rotodynamic pumps guideline for NPSH margin. https://webstore.ansi.org/standards/hi/ansihi2024-2610556
  9. International Organization for Standardization [ISO]. (2007). ISO 8501-1:2007, Preparation of steel substrates before application of paints and related products — Visual assessment of surface cleanliness — Part 1: Rust grades and preparation grades of uncoated steel substrates and of steel substrates after overall removal of previous coatings. https://www.iso.org/standard/43426.html
  10. International Organization for Standardization [ISO]. (2012a). ISO 19840:2012, Paints and varnishes — Corrosion protection of steel structures by protective paint systems — Measurement of, and acceptance criteria for, the thickness of dry films on rough surfaces. https://www.iso.org/standard/59523.html
  11. International Organization for Standardization [ISO]. (2012b). ISO 8503-1:2012, Preparation of steel substrates before application of paints and related products — Surface roughness characteristics of blast-cleaned steel substrates — Part 1: Specifications and definitions for ISO surface profile comparators for the assessment of abrasive blast-cleaned surfaces. https://www.iso.org/standard/51979.html
  12. Iwai, Y., & Nambu, K. (1997). Slurry wear properties of pump lining materials. Wear, 210(1–2), 211–219. https://doi.org/10.1016/S0043-1648(97)00055-0
  13. Morcillo, M. (1999). Soluble salts: Their effect on premature degradation of anticorrosive paints. Progress in Organic Coatings, 36(3), 137–147. https://doi.org/10.1016/S0300-9440(99)00036-3
  14. Tarodiya, R., & Gandhi, B. K. (2017). Hydraulic performance and erosive wear of centrifugal slurry pumps – A review. Powder Technology, 305, 27–38. https://doi.org/10.1016/j.powtec.2016.09.048
  15. Tarodiya, R., & Gandhi, B. K. (2019). Experimental investigation of centrifugal slurry pump casing wear handling solid-liquid mixtures. Wear, 434–435, 202972. https://doi.org/10.1016/j.wear.2019.202972
  16. U.S. Department of Energy [DOE]. (2006). Improving pumping system performance: A sourcebook for industry (2nd ed.). Industrial Technologies Program and Hydraulic Institute. Retrieved November 2026. https://www.energy.gov/sites/prod/files/2014/05/f16/pump.pdf
  17. Wood, R. J. K. (2006). Erosion–corrosion interactions and their effect on marine and offshore materials. Wear, 261(9), 1012–1023. https://doi.org/10.1016/j.wear.2006.03.033

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.