Washing parts again or replacing the whole quench oil is the usual response to staining after quenching, but unless it is clear whether the staining material formed or stayed behind in the tank, the washer or the tempering furnace, the same stains come back. What actually lies behind them can be oxidised quench oil, poor washing, oil residue baked on in tempering, leftover polymer film or water in the oil, and sometimes two or more at once.
Background
A basket comes out of tempering with brown patches on some parts and a dull brown film over the whole of others. Even with hardness inside the specification, parts that fail visual inspection must be washed again or shot blasted, and a customer who reads appearance as a sign of quality simply sends them back. The same spots can also end up where rust starts. Soil not removed before heat treatment is baked onto the surface and becomes a starting point for staining and corrosion, and alkaline cleaner left behind by poor rinsing can bring on rust (MacKenzie, 2024b).
The colour left on a part after quenching comes from one of two places. One is a film formed when something left on the surface, such as oil, cleaner or polymer, changes or bakes on under heat. The other is a thin oxide film grown on the steel itself in air; its colour comes from light interfering within the film according to its thickness, and it moves from brown towards purple and blue as the temperature rises (Peet & Bhadeshia, n.d.).
The first kind is solved only by tracing where the material formed or stayed behind: the quench tank, the washer or the tempering furnace. Residue problems of this kind usually show only after tempering, so the step where a stain is noticed and the step where it began can be different (MacKenzie, 2025).
In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: set aside a few stained and a few clean parts, find whether the stain first appears straight after quenching, after washing or after tempering, and then compare that lot's quenchant, washer bath and tempering conditions with each product's technical data sheet, the TDS, and the process standard.
Hypothesis 1: oxidised quench oil
Suspect this first in a quench tank that has been topped up for years without a change, on a line where heavier loads keep the oil hot for longer, and in a tank whose fouled heat exchanger no longer cools the oil well. Picture the time when the oil has turned darker than it used to be and sticky brown deposits have begun to cling to the tank walls and floor. Parts from that tank show brown stains spread in streaks, and washing does not take all of them off.
Quench oil takes oxygen from the air and heat together every time a hot part goes in. The oxidation rate roughly doubles with every 10°C rise, and once oxidation starts it keeps speeding up. Its products link up through condensation reactions into large molecules that no longer dissolve in the oil, and these become sludge on the tank floor and varnish on the parts, a thin brown film baked onto the surface. For most quench oils, a total acid number, the measure of acid content, above 1.5 to 2.0 mg KOH/g is read as a sign of staining or deposits on parts (MacKenzie, 2018a). In one experiment, cooling ability rose to a peak while peroxides built up during oxidation, and from that point viscosity and sludge began to increase and cooling ability fell again as polymerisation went on (Tagaya & Tamura, 1958). Oxidised oil shows higher viscosity and striped stains on parts, and soot carried in from a carburising atmosphere leaves stains that look identical to oxidation stains (MacKenzie, 2018b).
The state of the oil is known only by sampling and testing it. Viscosity, acid number, precipitation number for sludge, water and the cooling curve are the tests used to judge the quality and ageing of quench oil (ASTM International, 2021), and acid number is measured by potentiometric titration (ASTM International, 2024). A trend against the new-oil values and earlier analyses says more than any single figure. Look for sticky deposits on the tank walls, the floor and the heat exchanger surfaces, and check the records for whether the striped stains appeared when the analysis values began to rise.
When the analysis points to oxidation, decide with the oil supplier on a partial or full change and scoop the sludge off the floor. If the conditions that drove the oxidation stay as they are, though, the new oil goes the same way. Clean the heat exchanger to bring the oil temperature back, filter continuously to take out sludge and soot, and cut the coolant and cleaner that ride in on the parts. Residue on parts aggravates oxidation, and continuous filtration is recommended over periodic clean-outs (MacKenzie, 2018b).
Hypothesis 2: poor washing
Washing sits at two points: before quenching, to remove cutting fluid and chips, and after quenching, to take the oil off before tempering. Look this way when the washer bath has lost concentration or temperature, when the rinse water has not been changed for a long time, when washing time was cut to keep up with output, and when parts are packed so tightly in the basket that some spots never meet the liquid. Say washing time was shortened in a week when orders piled up. After tempering, stains gather only around holes and grooves, and the flat faces are clean.
Washing is two jobs: lifting off oil and soil, and rinsing the cleaner away again. If either falls short, something stays on the surface and is baked onto it at heat-treating temperature. Rinsing in particular is named as the critical step against cleaner residue (MacKenzie, 2024b). In one investigation of parts discoloured after tempering, a solvent wash of the surface yielded an oily residue, and the solids in the quench oil held chips and cooked cleaner residue (MacKenzie, 2025). The same investigation found the oil itself only slightly oxidised, so the cause was judged to be washing rather than the oil, and it also reported silicate cleaner carried into the rinse tank and dried as a yellow solid on rinsed parts. The same article explains that residue drying on parts can fuse with the surface at heat-treating temperature and leave chemical burn marks.
Look at parts straight out of the washer first. Wipe with a white cloth to see whether oil comes off, splash on water to see whether it spreads evenly over the surface, and check holes and grooves for trapped liquid or powder. Compare the washer bath concentration and temperature and the state of the rinse tank with the cleaner's TDS, and find in the records when the rinse water was last changed. Note too whether stains gather at particular spots in the basket or where parts are packed most densely.
With the cause narrowed to washing, bring the washer bath back within the TDS concentration and temperature ranges, and set a contamination limit for the rinse tank so the water is changed when it is reached. Dry the surface fully after rinsing, and hold washing time at a fixed value that is not cut when output piles up. Load baskets with enough space for the liquid to reach every face, and turn parts with many holes so the liquid drains.
Hypothesis 3: baked-on oil residue
Put this hypothesis at the front when parts go straight to tempering without washing after quenching, when their shape holds oil, as with blind holes and threads, and when parts are stacked so oil is trapped between touching faces. A case in point: shafts with threads and blind holes are oil-quenched in layers in a basket and, on a busy day, put into the tempering furnace unwashed. Acrid smoke rolls out when the door opens, and dark brown marks are left where parts touched and around the holes.
At tempering temperature, oil left on a part meets air and heat together. As the oil oxidises, its products link up through condensation and form varnish on the part (MacKenzie, 2018a), and dried residue can fuse with the surface at heat-treating temperature and leave burn marks. In the investigation mentioned above, the discolouration followed the outline of the neighbouring part and pointed to where parts had nested together (MacKenzie, 2025). What is easily confused with this is temper colour. Tempering in air grows a thin oxide film on the steel, whose thickness makes light interfere and gives it colour; on a specimen with a temperature gradient the colours run from brown at the cooler end through several shades to pale blue, consistent with the tempering temperature (Peet & Bhadeshia, n.d.). An oxide film forms over the whole surface according to temperature, whereas burnt oil forms where oil was left.
Where the stains sit is the first clue. Note whether they gather where oil would have pooled, such as touching faces, around holes and threads and on the underside of parts, or whether the whole part is an even colour. Wipe the stained area with a solvent-dampened cloth to see whether anything comes off, and check the tempering furnace records for temperature and exhaust. Split one lot in two and temper one half washed and the other as it is; that shows at once whether oil is the cause.
If burnt oil is confirmed, never skip washing the oil off before tempering, and load oil-holding shapes tilted or turned so the oil runs out. Use dividers or fixtures so parts do not nest, and check that the tempering furnace exhausts enough to clear the smoke. If it turns out to be an even temper colour rather than a stain, and appearance matters for the part, review a tempering atmosphere that limits the oxide film with the furnace supplier.
Hypothesis 4: leftover polymer film
This one belongs only to lines using a water-based quenchant with polymer dissolved in it, polyalkylene glycol, or PAG, in particular. It shows up when evaporation has raised the concentration, when poor cooling has let the bath run warm, and when parts go to tempering without a rinse after quenching. Take a summer afternoon when the quench tank cooling cannot keep up and the bath is warmer than usual, and parts are taken out and moved straight to the tempering furnace. A sticky film can be felt on the surface, and when tempering ends there are brown and black marks and a pungent smell from the furnace.
PAG has inverse solubility: at high temperature it no longer dissolves in water. When a hot part goes in, polymer comes out of solution as a thick film on its surface and controls the cooling rate, and as the part nears bath temperature the film breaks up and dissolves back into the bath. The higher the concentration, the thicker the film, and parts removed above the cloud point, the temperature at which the solution starts to split into two layers, carry out far too much polymer. Corrosion inhibitor in the bath also protects quenched parts only briefly, so they need their own protection after tempering (MacKenzie, 2024a). If such a film is tempered as it is, the polymer leaves a carbonaceous film and gives off acrid fumes, while an agitated rinse in water at room temperature is usually enough to remove it (MacKenzie, 2024b).
Start by measuring bath concentration with a refractometer against the TDS range, and check that the bath temperature sits well clear of that product's cloud point. The tests for judging the quality and ageing of water-based polymer quenchants are also set out in a standard guide, which can serve as the basis when routine analysis is left to the supplier (ASTM International, 2025). Touch parts just taken out to feel for a sticky film, and temper rinsed and unrinsed parts together to compare the staining.
If polymer film is the cause, the most direct fix is a water rinse between quenching and tempering. Measure concentration at fixed intervals and keep it in range, and work on the cooling so the bath stays below the cloud point. After rinsing and tempering, give parts a rust preventive before the next process or storage so that rust stains do not form.
Hypothesis 5: water in the oil
Water has more ways into quench oil than one might expect. Water-cooled heat exchangers are named as the biggest culprit, and water-cooled doors, fans and bearings, compressed air lines, water-containing fire-resistant hydraulic fluid, leaking roofs and water left in reclaimed oil all contribute (Frennea, 2018). Imagine a week of monsoon rain with drip marks under a roof seam above the quench tank. From then on, some parts of the same steel grade come out with stains and with patches of uneven hardness.
Quench oil dissolves very little water. Saturation for conventional quench oils is about 1,000 ppm, or roughly 0.1%, and even below 500 ppm, low-hardenability steels can develop soft spots and non-martensitic structures. Water above saturation turns to steam around the hot part and expands, pushing the oil up and raising the risk of fire and explosion (Frennea, 2018). Where water boils first on the part surface, cooling differs from the rest, so hardness variation and surface stains can appear together. Condition-monitoring guidance for quench oil also points out that water in the oil can bring soft spots, uneven hardness, staining and fires, and water in quench oil is usually held below 0.1% (Webster et al., n.d.).
Checking begins with a water measurement. The crackle test, listening for spitting as the oil is heated, is simple but unreliable and mostly catches water above 1,000 ppm, so Karl Fischer titration is needed to see down below 50 ppm (Frennea, 2018). Also take a sample near the tank floor to see whether water has settled. If water is high, work through a pressure test of the heat exchanger, leaks in the roof and pipework, and any change in cooling water use, and check the records for whether stains and soft spots coincided with rainy days or equipment maintenance.
Once water is confirmed, close the way it came in first. Drain water settled at the bottom, and agree a dewatering method with the oil supplier to bring the rest back within range. Water above saturation sharply raises the risk of fire and explosion, so consider stopping quenching in that tank until the water content is back in range. From then on, make water a routine analysis item, and test more often in the wet season and after heat exchanger maintenance.
Finding the cause
The five hypotheses do not need to be investigated all at once. Catching the step at which the stain first appears is the easiest check and rules out the most. Set aside a few parts straight after quenching, after washing and after tempering, and compare them. If the stain is already there after quenching, look at the quench oil: oxidised oil or water in the oil. If it first shows after tempering, ask whether oil residue or polymer film burnt on, or whether it is simply the temper colour of an oxide film. Washing residue also usually shows only after tempering, though, so a stain seen after tempering does not clear the washer (MacKenzie, 2025).
Next is the shape of the stain. An even colour over the whole part that matches the tempering temperature points first to an oxide film. Striped stains spread across parts from the same tank point to oil oxidation, but soot stains look the same, so the eye cannot separate them and an oil analysis is needed (MacKenzie, 2018b). Stains gathered on touching faces and around holes and threads point to oil residue or washing, a sticky film with a pungent smell to polymer film, and stains together with soft spots to water in the oil.
If that still does not settle it, move on to analysis. Measure viscosity, acid number, precipitation number and water for quench oil and concentration for a water-based quenchant, and collect residue from the stained area with solvent for infrared spectroscopy, FTIR, to tell oil from cleaner. The investigation mentioned earlier did just this, comparing the residue with tank sludge and adding an oil analysis to show that the cause lay in washing (MacKenzie, 2025).
The final check is a control trial that changes one thing. Split a lot in two and, for one half only, wash once more, quench a few parts in a small container of fresh oil, or add a rinse after quenching. Change only one thing at a time, or there is no telling what removed the stain. Afterwards, count the share of stained parts against the agreed appearance standard in the same way as before, and the job is done only when that share is back to its usual level.
The hypotheses can also be tangled together. When poor washing lets cutting fluid and cleaner into the quench oil, the oil oxidises faster (MacKenzie, 2018b), and the sludge from oxidation coats the heat exchanger and pushes the oil temperature up further. In a tank with water in it, the stains and the fire risk grow together. In such cases, close the ways contamination gets in, such as water and washing, before changing or re-examining the oil, because with those left open the new oil will make the same stains again.
Limits and cautions
Control ranges for acid number, water, concentration and washer conditions differ by oil, quenchant and cleaner, so numeric decisions follow the product's TDS and the supplier's guidance. Appearance acceptance follows the standard agreed with the customer, and where hardness variation is suspected alongside the stains, confirm it by hardness testing and metallographic examination. Residue analysis is laboratory work, and for safety-related parts, do not release on floor judgement alone; get the quality engineer to confirm.
Safety matters too. Fire prevention and safety devices for furnaces with oil quench equipment are covered by safety standards for furnaces and quench systems, so modifications to tanks and furnaces or changes to operating conditions follow that standard and the equipment supplier's instructions (NFPA, 2023). Water in quench oil can lead to fire and explosion, so a high water reading is never brushed aside. Extract fumes from tempering by ventilation, and for quench oil, water-based quenchant and cleaner, wear protective equipment as set out in each product's safety data sheet, the SDS. When sampling beside hot tanks and parts, wear heat-resistant gloves and eye protection.
Sources
- ASTM International. (2021). ASTM D6710-21, Standard guide for evaluation of hydrocarbon-based quench oil. https://store.astm.org/d6710-21.html
- ASTM International. (2024). ASTM D664-24, Standard test method for acid number of petroleum products by potentiometric titration. https://store.astm.org/d0664-24.html
- ASTM International. (2025). ASTM D6666-25, Standard guide for evaluation of aqueous polymer quenchants. https://store.astm.org/d6666-25.html
- Frennea, R. (2018). Water in oil-based quenchants can be problematic. Gear Solutions. https://gearsolutions.com/departments/hot-seat/water-in-oil-based-quenchants-can-be-problematic/
- MacKenzie, D. S. (2018a). Oil quenchants – Understanding the chemistry (Part III). Gear Solutions. https://gearsolutions.com/departments/oil-quenchants-understanding-the-chemistry-part-iii/
- MacKenzie, D. S. (2018b). Corrective actions for degraded quench oil. Gear Solutions. https://gearsolutions.com/?p=33624
- MacKenzie, D. S. (2024a). Polymer quenchants – Polyalkylene glycol quenchants. Gear Solutions. https://gearsolutions.com/departments/hot-seat/polymer-quenchants-polyalkylene-glycol-quenchants
- MacKenzie, D. S. (2024b). Cleaning for heat treatment – Part II. Thermal Processing. https://thermalprocessing.com/?p=29459
- MacKenzie, D. S. (2025). Cleaning for heat treatment – Part IV. Thermal Processing. https://thermalprocessing.com/?p=29811
- National Fire Protection Association [NFPA]. (2023). NFPA 86, Standard for ovens and furnaces.
- Peet, M., & Bhadeshia, H. K. D. H. (n.d.). Oxide on steel and tempering colours. University of Cambridge, Phase Transformations Group. Retrieved November 2026. https://www.phase-trans.msm.cam.ac.uk/2008/Oxide/Oxide.html
- Tagaya, M., & Tamura, I. (1958). Changes of cooling ability with oxidation and polymerization process of oil: On the deterioration of quenching oils-IV. Tetsu-to-Hagane, 44(6), 668–673. https://doi.org/10.2355/tetsutohagane1955.44.6_668
- Webster, G. M., Totten, G. E., & Wachter, D. A. (n.d.). Quenchant fundamentals: Condition monitoring of quench oils. Machinery Lubrication. Retrieved November 2026. https://www.machinerylubrication.com/Articles/Print/430