BlogApplication notes
Why does refrigerant dilute the compressor oil and wear the bearings?
- Type
- Application notes
- Published
- 23 November 2026
- Prepared by
- Jonghwan Moon
- Product group
- Equipment/Service Lubricants
Switching to a thicker oil is the usual response when refrigeration compressor bearings wear, but if refrigerant is what thinned the oil, a higher grade alone tends to end up thinned again. What actually lies behind it can be low mixture viscosity from dissolved refrigerant, foaming at start-up, a crankcase heater that is off, overcharge or liquid returning through low superheat, and sometimes two or more at once.
Background
Open the refrigeration compressor and the bearing surfaces on the crankshaft show long score marks, yet the drained oil is clear and looks fine. At every start the sight glass fills white with foam and a brief knocking dies away. Replace the bearings, run again, and a few months later the same places are worn.
Worn bearings end in compressor failure, and while the refrigeration plant is down, the cold store or process cannot hold its temperature. Sometimes the whole compressor has to be replaced. When crankcase oil is diluted by liquid refrigerant, its viscosity and lubricity fall, parts lubricated by the oil such as the main and connecting rod bearings wear excessively, and compressor life is shortened (Barbier, 2003).
Refrigeration oil is chosen to mix well with the refrigerant, because that is how it travels round the system and back to the compressor. The price is that some refrigerant is always dissolved in the oil, and the more that dissolves, the lower the mixture's viscosity. Measurements on HFC-134a with POE oil also showed viscosity falling as refrigerant dilution rose (Cavestri, 1993). More dissolves at higher pressure and lower temperature, so even with the same oil, the viscosity that actually reaches the bearings varies widely with running conditions and standstill time. As viscosity and oil film thin, the moving parts that bear on each other can be damaged (Brostrom et al., 2020).
In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: gather when the bearings wore and the running records over that period, namely standstill times and number of starts, suction pressure and superheat, crankcase temperature and charging history, and compare them with the compressor maker's limits and the viscosity grade in the oil's technical data sheet, the TDS.
Hypothesis 1: low mixture viscosity
If bearing wear increased after a change of refrigerant or oil, look first at how the two suit each other. It applies when the refrigerant was converted but the old oil was kept, when a lower viscosity grade went in, and when long spells of running combine high suction pressure with low oil temperature. Take a plant converted to a low global warming potential refrigerant as an example. Running pressures and temperatures are in the normal range and stops are not long, yet oil drained at service shows more bearing metal than before.
The better refrigerant dissolves in the oil, the thinner the mixture. The measured drop is not small. Conventional POE oils mixed with R-32 or R-410A lost as much as 25 to 54% of their viscosity under normal compressor conditions, and the dilution was greater with R-32. The same study reports that POE redesigned for R-32 in how its solubility relates to its viscosity avoided this loss (Urrego Leon et al., 2014). Even at the same viscosity grade, how much refrigerant dissolves depends on the oil's structure, and viscosity can fall almost in a straight line with dilution or bend sharply at a certain concentration (Cavestri, 1993). What the bearings receive is not the viscosity in the drum but that of the mixture with refrigerant dissolved in it, so once that value drops below the minimum the bearings need, the film thins and metal starts to touch metal.
First confirm that the refrigerant and oil in use appear together on the compressor maker's approved list. Give the oil supplier the suction pressure and oil temperature in service, obtain solubility and viscosity data for the mixture viscosity at those conditions, and compare it with the compressor maker's minimum. Kinematic viscosity of drained oil measured in a laboratory shows the state of the oil itself, such as mixing with another grade or degradation, rather than the mixture viscosity in service, because the refrigerant has already escaped (ASTM International, 2026a). Analyse the same sample for wear metals such as iron, copper, aluminium and tin, and keep the trend (ASTM International, 2026b).
If the mixture viscosity comes out short, change to an oil chosen for that refrigerant. Simply moving up one grade may not solve it, because an oil in which the refrigerant dissolves more readily thins out again in service even at a higher grade. Use a pairing agreed between the compressor maker and the oil supplier, and review running conditions so that spells of very low oil temperature do not persist. After the change, watch whether the wear metal trend comes down.
Hypothesis 2: start-up foaming
In some machines the odd noise and the foam are concentrated in the brief moments right after a start. Look at this hypothesis for the first start after a long stop, the morning start of a machine idle overnight, and operation that starts and stops at short intervals. Picture a winter morning as a compressor idle all night begins to turn. The sight glass fills with foam in an instant so the oil level cannot be read, a metallic noise lasts a short while, and it fades as the foam settles.
Refrigerant that dissolved heavily in the oil during standstill comes out as bubbles when the crankcase pressure drops suddenly at start-up. Experiments depressurising refrigerant and oil mixtures observed bubbles forming and growing, then foam building up and collapsing, with the maximum foam height and lifetime depending on the initial refrigerant content and the temperature (Fortkamp & Barbosa, 2015). A study of start-up foaming in rotary compressors found that the motor rotor, the vane and the discharge refrigerant flow churned the mixture into foam, and the degree of foaming tracked how readily the refrigerant dissolved in the oil and how much refrigerant was in the churned part of the liquid (Yanagisawa & Shimizu, 1986). Foamed oil drawn in by the pump or oil holes cannot form a proper film, and some is carried out with the discharge gas so the oil level falls. Starting at full speed with liquid refrigerant in the sump can starve the parts of lubrication through oil dilution or damage them as the compressor tries to compress liquid (Tolbert et al., 2014).
Watching the moment of start-up directly is the best check. At the first start after a long stop, record the foam height in the sight glass and how long it takes to settle, how far the oil level drops and recovers, and note noise and vibration too. On compressors with an oil pump, see whether oil pressure builds in time just after start and whether there are trips on low oil pressure. Comparing whether foaming worsens with longer stops and a colder crankcase during standstill shows how much is down to dissolved refrigerant.
If foaming is the problem, the root fix is to cut the refrigerant that dissolves in the oil during standstill. Bring the crankcase heater back into service, give the oil time to warm before starting, and follow the maker's recommended shutdown method if there is one. For variable-speed compressors, review a slow ramp-up at start with the maker. If short starts and stops are frequent, adjust the control settings to cut the number of starts.
Hypothesis 3: crankcase heater off
There are times when the compressor becomes the coldest point in the system: an outdoor compressor standing for long periods in winter, a unit switched off at the breaker for the off-season and switched back on, a heater disconnected to save energy, or a heater that has burned out without anyone noticing. Consider a rooftop refrigeration unit whose breaker was off all off-season and is switched back on in spring. The breaker goes up, the unit is started straight away, the compressor starts noisily, and oil sloshes in the sight glass, filled higher than usual.
After shutdown, refrigerant vapour from the compressor housing and elsewhere in the system can migrate into the oil sump or condense there, forming a mixture of liquid refrigerant and oil. A crankcase heater is fitted to keep the sump warm so the liquid refrigerant evaporates, though it is also pointed out that it must stay on and draws considerable power, lowering efficiency (Tolbert et al., 2014). If the heater is not working, the sump cools to the surrounding temperature, and cold oil draws in more refrigerant. The longer the stop, the more builds up, and oil standing higher than usual in the sight glass may be that extra refrigerant. Start in that state and the foaming and thin oil described above reach the bearings all at once.
Start by checking that the heater actually receives power. During a stop, measure heater current with a clamp meter and take the surface temperature at the bottom of the sump with a contact thermometer to confirm it is warmer than nearby piping and the air. Check that the heater is not wired so that it switches off when the compressor stops, and that the breaker has not been turned off for the off-season, taking the heater with it. If the oil level repeatedly rises during stops and then drops with foaming after start-up, this hypothesis is likely.
If the heater is the cause, replace a burned-out heater and correct the wiring so it is on during stops. For a machine that has been without power for a long time, switch the heater on first for the time the maker specifies to warm the oil before starting. Rather than disconnecting the heater to save energy, discuss with the maker whether a control that runs the heater only when needed is available. Keeping an outdoor compressor out of direct cold wind also helps.
Hypothesis 4: overcharge
Suspect overcharge in a machine whose refrigerant has been topped up by pressure readings without weighing the charge. Typical cases are repeated top-ups after leak repairs without recovering the charge, filling to suit high midsummer pressures, and a miscalculated extra charge for pipe length. Here is a machine that several service contractors have topped up in turn over a few years. Nobody has compared the nameplate charge with what is now in the system, and its condensing pressure always reads higher than other machines in the same season.
With too much refrigerant, the surplus liquid backs up in the condenser and subcooling and condensing temperature rise. In tests on a heat pump with a thermostatic expansion valve charged 10 to 30% above the correct amount, liquid line subcooling and condenser saturation temperature rose steadily with the overcharge, while the compressor discharge wall temperature fell (Kim et al., 2006). A falling discharge temperature can mean the gas entering the compressor carries less superheat, and one diagnostic method treats actual discharge superheat below the theoretical value as a sign of liquid returning (Brostrom et al., 2020). Moreover, the more refrigerant the system holds, the more can migrate into the sump and dissolve there during stops, so overcharge makes the foaming and heater problems above worse.
Go back through the charging history first. Gather the nameplate or design charge, the extra for pipe length and every top-up since, and estimate how much is in the system now. While running, measure liquid line subcooling and condensing pressure against the maker's reference values, and work out discharge superheat from discharge temperature and the condensing temperature at the time. If subcooling is clearly above the reference and condensing pressure is higher than similar machines under similar conditions while the condenser is clean, lean towards too much refrigerant.
If overcharge is confirmed, recover all the refrigerant with recovery equipment and recharge the amount set by the nameplate and pipe length, weighed on scales. Bleeding off by pressure alone tends to drift wrong again. After recharging, check subcooling and superheat against the reference values, and record every later top-up by weight. If top-ups were often needed, find and fix the leak that caused them first.
Hypothesis 5: low superheat
If frost or condensation forms on the compressor suction line and the lower part of the housing while running, check whether liquid that did not finish evaporating in the evaporator is coming back. This happens when evaporator fans are blocked or stopped, when the expansion valve sticks or is set wrongly, right after defrost, and when the evaporator air filter is clogged or the coil is heavily frosted. Take the moment just after defrost ends in a cold store. The suction line is frozen white right up to the compressor inlet, droplets form on the lower shell, and the compressor makes a dull sound unlike its usual one.
Liquid coming back into the suction line is called liquid floodback. It can arise from blocked evaporator fans, stuck or malfunctioning expansion valves and defrost cycles, and when severe it can raise oil dilution to an unacceptable level, reducing viscosity and the oil film thickness between mating moving parts and damaging them (Brostrom et al., 2020). Another source lists a wrong expansion valve setting or a valve fault, clogged evaporator air filters and frost, and fan failure as causes, and explains that liquid refrigerant entering the crankcase thins the oil so the main and connecting rod bearings wear excessively. The same source holds that superheat measured at the compressor suction inlet shows whether liquid is coming back (Barbier, 2003). Superheat says how far the suction gas has been heated above the saturation temperature at its pressure, so the closer it gets to zero, the more room there is for liquid to come in with the gas.
Measure superheat close to the compressor suction inlet. Convert suction pressure to the refrigerant's saturation temperature, take the pipe surface temperature at the same point with a contact thermometer, and find the difference. Do not measure just once; log it under changing conditions such as right after defrost, at light load at night and with a fan stopped. Work out discharge superheat as well from discharge and condensing temperatures, and see whether it falls when suction superheat is low. Check evaporator fans, air filters, frost and the expansion valve's sensing bulb mounting and setting by eye.
Correct whatever is driving superheat down first. Repair stopped fans, clear clogged filters and heavy frost, re-secure a loose expansion valve sensing bulb, and set the valve to the superheat the maker specifies. Replace a valve that sticks or has failed. If liquid comes back after every defrost, adjust the defrost termination and the point at which the fans restart, and review with the maker whether a suction accumulator to hold back liquid is needed.
Finding the cause
Of the five hypotheses, start with what can be seen without stopping the machine. Heater current and sump temperature, suction and discharge superheat, subcooling and condensing pressure only need instruments applied while it runs or stands. Charging history and whether the oil and refrigerant are approved can be confirmed on paper. Recovering and reweighing the charge or changing the oil comes after the earlier checks have narrowed the cause.
When the symptoms appear is the first clue. If noise and foam cluster around standstill, such as starts after long stops, in winter or after the off-season, look first at start-up foaming and a heater that is off. Frost on the suction line and noise while running point to liquid returning through low superheat; condensing pressure and subcooling above the reference in service, with a clean condenser, point to overcharge. If wear metals increased after a change of refrigerant or oil without any of these signs, lean towards mixture viscosity reduced by dissolved refrigerant.
Oil analysis backs up the judgement. Whether wear metals rise at each service, and whether kinematic viscosity has shifted through mixing with another grade, separates a problem in the oil itself from one in the running conditions. But refrigerant escapes from drained oil, so a normal laboratory viscosity does not mean the mixture viscosity in service was sufficient.
Once the cause has narrowed, change one thing at a time. Restore the heater and allow warm-up before starting, then see whether start-up foaming eases; reset the expansion valve and see whether superheat steadies; correct the charge and see whether subcooling returns to its reference. Only by changing one thing at a time can the effect be traced. The job is done only when foam and noise at start-up are gone, superheat stays within the maker's range and the next oil analysis shows the rise in wear metals has stopped.
The hypotheses feed one another. In an overcharged system with the heater also off, more refrigerant migrates into the sump during stops, and start-up foaming grows to match. Add low superheat that lets liquid return in service, and the oil stays thin both at rest and running. In such cases, first fix the routes by which refrigerant reaches the sump, namely charge, heater and superheat, and then check whether the refrigerant and oil suit each other. Raising the oil grade first can merely slow the wear while hiding the cause.
Limits and cautions
Minimum viscosity, suitable superheat and subcooling, charge and heater warm-up time differ with each combination of compressor, refrigerant and oil, so numeric decisions follow the compressor and equipment makers' guidance and the oil's TDS. Change the refrigerant and oil pairing only within what the compressor maker has approved. Refrigerant recovery and charging are for technicians qualified to handle refrigerants, working under local regulations, and refrigerant is never vented.
Heater and wiring checks are for qualified electricians, with power isolated and locked out. On a running compressor the discharge line is hot and the suction line may be frozen, so wear gloves, and wear eye protection when sampling oil from a pressurised system, since refrigerant can spray out with it. Handle oils and refrigerants according to the product's safety data sheet, the SDS, and follow the maker's separate safety procedures for systems using flammable refrigerants.
Sources
- ASTM International. (2026a). ASTM D445-26, Standard test method for kinematic viscosity of transparent and opaque liquids (and calculation of dynamic viscosity). https://store.astm.org/d0445-26.html
- ASTM International. (2026b). ASTM D5185-26, Standard test method for multielement determination of used and unused lubricating oils and base oils by inductively coupled plasma atomic emission spectrometry (ICP-AES). https://store.astm.org/d5185-26.html
- Barbier, W. J. (2003). Rate of change detector for refrigerant floodback (U.S. Patent No. 6,578,373). U.S. Patent and Trademark Office. https://patents.google.com/patent/US6578373B1
- Brostrom, T. R., Kamat, R., Winandy, E., & Bertagnolio, S. (2020). Compressor floodback protection system (U.S. Patent No. 10,801,762). U.S. Patent and Trademark Office. https://patents.google.com/patent/US10801762B2
- Cavestri, R. C. (1993). Measurement of viscosity, density, and gas solubility of refrigerant blends in selected synthetic lubricants: Quarterly report, July 1 to September 30, 1993 (DOE/CE/23810-22C). Air-Conditioning and Refrigeration Technology Institute. https://www.osti.gov/servlets/purl/10195409
- Fortkamp, F. P., & Barbosa, J. R., Jr. (2015). Refrigerant desorption and foaming in mixtures of HFC-134a and HFO-1234yf and a polyol ester lubricating oil. International Journal of Refrigeration, 53, 69–79. https://doi.org/10.1016/j.ijrefrig.2015.01.015
- Kim, M., Payne, W. V., Domanski, P. A., & Hermes, C. J. L. (2006). Performance of a residential heat pump operating in the cooling mode with single faults imposed (NISTIR 7350). National Institute of Standards and Technology. https://nvlpubs.nist.gov/nistpubs/ir/2006/ir7350.pdf
- Tolbert, J. W., Jr., Moody, B. A., Chumley, E. K., Denzau, R. C., Edwards, J. D., Gilliam, D. R., Hix, S., Toner, J. M., Trent, M. R., Wampler, T. M., & Williams, J. R. (2014). System and method for starting a compressor (U.S. Patent No. 8,672,642). U.S. Patent and Trademark Office. https://patents.google.com/patent/US8672642B2
- Urrego Leon, R. A., Benanti, T. L., & Hessell, E. T. (2014). Solution properties of polyol ester lubricants designed for use with R-32 and related low GWP refrigerant blends. In International Compressor Engineering Conference (Paper 1491). Purdue University. https://docs.lib.purdue.edu/icec/2355
- Yanagisawa, T., & Shimizu, T. (1986). Foaming of refrigerating oil in a rolling piston type rotary compressor. International Journal of Refrigeration, 9(1), 17–20. https://doi.org/10.1016/0140-7007(86)90145-3