KALTECKOREA

BlogApplication notes

Why do cold-rolled coils stain in annealing?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Metalworking Fluids (MWF)

Adjusting furnace temperature and time is the usual response to stains after annealing, but if what forms the stain was carried onto the coil from the mill, changing the furnace alone will not remove it. What actually lies behind it can be too much residual oil, low-volatility components, iron fines, the wrong furnace atmosphere or an unstable emulsion, and sometimes two or more at once.

Background

A coil comes out of the batch annealing furnace, and when it is uncoiled, brown or black bands run along the strip edges and grey stains spread here and there across the middle. Stained coils have to be cleaned again or downgraded, and if they go on to a plating or painting line as they are, they carry the seeds of poor wetting and poor adhesion. Smudge at the edges of cold-rolled strip has been reported to resist conventional electrolytic cleaning and to cause dewetting of tinplate (Komai et al., 1981).

In cold rolling, an emulsion of rolling oil dispersed in water is sprayed onto the rolls and strip to lubricate and cool them (EPA, 2002). The rolled strip carries a thin oil film and iron particles generated in rolling, and batch annealing heats this strip, still wound as a coil, in a protective gas. The remaining oil has to evaporate or decompose and leave during heating, and in a thermogravimetric study its removal depended on the nature of the furnace gas (Pillar et al., 2005). A European steel research project also treated iron fines and oil residues from cold rolling as a nuisance that follows the strip into later steps (European Commission, n.d.-a).

So annealing stains fall into two broad kinds: oil that could not get away and was left as carbon after heating, and oxidation of the steel surface by the furnace atmosphere. Iron particles take part in both. Where the stain sits across the strip width, in which laps of the coil and in which coil of the stack helps narrow the cause.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: cut samples from the same positions on a stained coil and a clean one, record where the stain sits, and compare that coil's rolling conditions, annealing cycle and emulsion analysis records with the rolling oil's technical data sheet, the TDS.

Hypothesis 1: too much residual oil

Residual oil on the strip changes when rolling conditions change. Look at this hypothesis first when emulsion concentration or the supply at the last stand has been raised to roll thin gauges, when the wipers or air nozzles that strip liquid off the strip are worn or blocked, and on lines that send coils to annealing without a separate cleaning step. Think of a week crowded with thin-gauge orders. The strip leaving the last stand looks oilier than usual, and only the coils rolled that week show broad brown stains towards the middle of the strip after annealing.

The amount of residual oil matters because oil does not all leave cleanly when heated. In a Korean study of batch annealing stains, the rolling oil from the mill contained about 40 ppm of carbonisable material and began to decompose thermally at about 220 °C. In the same study's annealing tests, there was almost no carbonisation at 200 °C, while carbonisation appeared above 240 °C (Lee, 2018). The more oil is left on the strip, the more of it decomposes, so there is more room for carbon to remain, and that is what shows as brown or black stains when the coil is unwound.

Numbers settle it fastest. Cut a set area from strip that has passed the last stand, wash it with solvent and weigh it before and after; the difference gives the residual oil, so stained and clean coils can be compared on the same basis. Match the condition of the wipers and air nozzles and the emulsion supply and concentration records for the last stand against the day the coil was rolled. If the stain covers only one side of the width rather than the whole strip, start with the nozzles and wipers on that side.

If residual oil turns out high, work on letting less oil leave the mill on the strip. Repair or replace the wipers and air nozzles, and bring emulsion concentration and last-stand supply back inside the TDS ranges, as far as lubrication allows. For products where residual oil stays high, alkaline cleaning can be added before annealing, and electrolytic cleaning is used where a cleaner surface is needed (EPA, 2002). Review the early heating rate and gas flow with the furnace maker.

Hypothesis 2: low-volatility oil

If the amount of oil is unchanged but stains appear, look at what the oil is made of. Typical times are after a change of rolling oil supplier or formulation, after a move to a rolling oil richer in fats or esters for better lubrication, after an additive is added, or after another oil has leaked into the emulsion tank. Annealing cycle and rolling conditions stay the same, yet from the month the new rolling oil went in, annealed strip takes on an even greyish cast. Rub the strip with a white cloth and a faint black mark comes off.

Rolling oil is a blend of components, and each one leaves at a different temperature and leaves behind a different residue when heated. A study that used thermogravimetry to mimic what rolling oil on the strip goes through in annealing found that triglycerides, the main component of fats, were a major source of high surface carbon among rolling oil raw materials, and it also screened contaminants common in rolling systems by their residue (Sech & Kleksiak, 1996). A study comparing vegetable-based rolling oils before and after heating by infrared spectroscopy, FT-IR, found evidence that the oils degraded on heating (Mogwaneng, 2008). Components that fail to leave and change on the strip are prone to decompose at higher temperatures and leave carbon.

To tell them apart, put the oil itself on the bench. Run thermogravimetry on fresh rolling oil and on oil separated from the in-use emulsion, and compare how much of each remains across the annealing temperature range. A simple test that spreads each oil thinly on clean strip and heats it in a gas close to the annealing atmosphere also gives surface colours to compare side by side. If only the in-use oil leaves much residue, suspect leaked-in oil or degradation; if fresh oil does too, look at the formulation.

If composition is the cause, rebalance lubrication against annealing cleanliness. The same study discussed additives that reduce residue and help the oil burn off cleanly (Sech & Kleksiak, 1996). When changing rolling oil, ask the supplier for annealing residue test data, and switch only after trial coils have been run through the plant's own annealing cycle. Stop hydraulic or gear oil leaks into the system, and skim off oil floating on the tank.

Hypothesis 3: too many iron fines

During rolling, very small iron particles come off as the strip stretches and slips against the rolls. This tends to happen when the share of high-strength steel has grown, right after new rolls with a rougher surface have gone in, in seasons when the emulsion runs cooler, and when maintenance of the magnetic separators or filters has fallen behind. For a few days after a roll change, the edges of annealed coils are noticeably darker than the middle, and tape pressed onto the strip and peeled off comes away with black powder.

Iron fines take part in staining in two ways. One is that the particles themselves stay on the surface as a stain. Smudge on cold-rolled strip for tinplate appeared to be a mix of iron and iron oxide powders, built up at the edges to more than twice the level at the centre, and grew with rolling speed and with reduction at the last stand, while supplying more oil there reduced it (Komai et al., 1981). The other is that they change the oil. The same study held that this smudge degrades palm oil, and in a laboratory mill study, more fines formed with rougher rolls, higher emulsion concentration and base oil viscosity, and lower emulsion temperature, while scum formed from the fines lowered emulsion stability and soiled the mill (Wang et al., 2025). As fines rose with growing high-strength steel output, a rolling oil that disperses them well was reported to improve mill and strip cleanliness (Inagaki et al., 2017).

Measure in two places, the strip and the emulsion. Lift samples from the edge and centre of rolled strip with tape, or wipe them with white filter paper, and compare the colour; that shows at once where the fines gather. Measure iron content in the emulsion at fixed intervals to follow the trend, and set it beside the records of roll changes, steel grade mix and emulsion temperature. Well-designed magnetic separators can hold iron in rolling solutions below 100 ppm (EPA, 2002), so if iron keeps climbing, check whether the separators and filters are doing their job.

Once the cause narrows to fines, act in two directions: make fewer and remove more. Shorten the cleaning intervals for the magnetic separators and filters, check the roughness and running-in of new rolls, and keep the emulsion temperature within the TDS range. If the share of high-strength steel will keep growing, trial a rolling oil with better fines dispersion with the supplier. On lines that clean the strip after rolling, review cleaning efficiency as well.

Hypothesis 4: wrong atmosphere

The stain may come from the furnace rather than the oil. Look at this hypothesis when moisture or oxygen in the protective gas has risen, that is, when purging is short, the inner cover seal leaks or the gas supply fluctuates, and in cycles where the coil edges get much hotter than the middle. Uncoil strip from a furnace whose cover seal is overdue for replacement: an iridescent or brown band is darkest along the strip edges and fades towards the middle.

How well a hydrogen and nitrogen protective gas guards the steel depends on the moisture and oxygen in it. A study that examined low-carbon strip batch annealed in 4% hydrogen under the electron microscope found that selective oxidation, where elements in the steel such as manganese oxidise at the surface first, was concentrated near the edges rather than spread across the width, with particles of manganese iron oxide and manganese chromium oxide forming along grain boundaries. These particles may explain a band of low reflectivity at the edge after plating, and the authors attributed the pattern to width-wise differences in dew point, the moisture or oxygen potential of the gas (Wilson et al., 2007). A European research project linked coloured edge staining to stronger selective oxidation at the edges, which reach higher temperatures during annealing, identified water vapour as the driver of this oxidation, and reported that pickling alone did not remove the difference between edge and centre (European Commission, n.d.-b).

Log the dew point of the protective gas through the whole cycle with a dew point meter, paying particular attention to early heating and the cooling stage. Leak-test the inner cover by the set method, and check purge time and gas flow against the records. If stains gather at the edges while the middle of the strip is clean, the case for atmosphere and temperature distribution grows stronger; compare whether the same pattern appears on other bases of the same furnace.

If the dew point runs high or the cover leaks, fix the furnace first. Seal leaks at the cover and gas lines, reset purge time against the dew point at the end of purging, and check the gas dryer. For a furnace with a large edge-to-centre temperature difference, the same project proposed reducing it with a high-convection pure hydrogen atmosphere (European Commission, n.d.-b), so adjust hydrogen share, convection fans and heating curve with the furnace maker. The atmosphere also affects how residual oil leaves; in thermogravimetry, a reducing atmosphere was the best environment for oil removal (Pillar et al., 2005).

Hypothesis 5: unstable emulsion

An emulsion keeps changing in service. Suspect it in a tank that has gone long without renewal, a tank with other oil mixed in, when make-up water hardness or temperature has changed, or when odour or foam has increased. A look down into an emulsion tank that has gone long without renewal shows a yellowish oil layer and brown scum floating on top, while the oil film on the strip beads up here and there. Coils annealed at that time come out with stains in a blotchy pattern, with no fixed position.

Plate-out, the way the emulsion turns into an oil film when it meets the strip, sets how much oil stays on it. In a study that measured plate-out over short times, the oil deposited grew with the time between emulsion supply and contact with the strip, and oil concentration and droplet size also changed the result (Kimura et al., 2009). So when droplet size and stability drift, the amount and evenness of oil on the strip drift with them. The dispersion stability of rolling oil is measured by a standard test method, and the standard itself notes that each mill needs a different degree of stability (ASTM International, 2022). The report that scum formed from fines lowers emulsion stability means iron fines and this hypothesis feed each other (Wang et al., 2025).

Spread out the emulsion analysis sheets. Measure concentration, droplet size, temperature, pH, iron and floating oil at fixed intervals, and see how fast oil rises when a tank sample is left to stand. Running the same tests on fresh rolling oil gives a baseline for how far the current emulsion has drifted from its starting state. Check whether the dates of the stains line up with the dates the analysis wandered.

Correct each cause of the drift in turn. Skim off floating oil and scum, trace leaking oil to its source and stop it, and keep make-up water hardness and temperature steady. Bring concentration and droplet size back into the TDS ranges, and if they still do not recover, agree with the supplier when to replace part of the tank with fresh emulsion.

Finding the cause

Five hypotheses do not mean five separate investigations. Start with what is already on record. Emulsion analysis sheets and furnace dew point logs can be read at a desk, and residual oil and fines on the strip can be measured on a few samples within a day. Thermogravimetry of the oil itself has to go to a laboratory, so it comes after.

The first clue is where the stain sits. Oxide bands concentrated along the strip edges match the reports on atmosphere and temperature distribution (Wilson et al., 2007), and dark edges with black powder on tape match the reports on iron fines (Komai et al., 1981). Stains spread across the middle or over the whole strip, away from the edges, call for a look at the amount and composition of the oil carried in first, and a blotchy pattern with no fixed position adds the emulsion to the list. Do not settle the cause on position alone; confirm it with timing and the control trials below.

Next is timing. Set the date the stains began beside the dates of rolling oil changes, roll changes, gauge changes, cover seal replacements and tank renewals. If coils from the same rolling go through a different furnace and the stain follows them, suspect the mill; if coils from another line out of the same furnace are stained too, suspect the furnace.

If that does not settle it, run control trials. Put two samples cut from the same coil into the same furnace, one as it is and one washed with solvent; if only the washed one comes out clean, the cause was carried in on the surface. Spreading fresh and in-use oil on clean strip and heating both through the same cycle separates composition from degradation. Change only one thing at a time, and afterwards count the share of stained coils on the same basis as before.

The hypotheses can overlap. More iron fines mean scum that unsettles the emulsion, an unsettled emulsion leaves oil unevenly on the strip, and that oil stains more readily in a furnace with a poor atmosphere. In such cases, stabilise the mill side first, emulsion and fines control, and then look at the furnace atmosphere, because while what the strip carries in keeps shifting, the effect of a change to furnace conditions cannot be compared fairly.

Limits and cautions

Suitable emulsion concentration, temperature, iron limits, annealing temperature and dew point, and hydrogen share differ by steel grade, rolling oil and furnace design, so numeric decisions follow the rolling oil's TDS and the furnace maker's guidance. Whether a stain is oxide or carbon, and which elements are enriched, is for a laboratory with surface analysis equipment to judge, and products with strict surface requirements, such as automotive outer panels or tinplate substrate for food cans, should not be released on floor judgement alone.

Safety matters too. Furnaces running a protective gas that contains hydrogen should handle purging, leak checks and emergency shutdown in line with the safety standard for ovens and furnaces (NFPA, 2023). Before lifting a cover or entering a furnace, check gas concentrations and follow lockout procedures. For rolling oils, cleaners and solvents, follow the product's safety data sheet, the SDS, for protective equipment and ventilation, and avoid breathing emulsion mist.

Sources

  1. ASTM International. (2022). ASTM D3342-22, Standard test method for dispersion stability of new (unused) rolling oil dispersions in water. https://store.astm.org/d3342-22.html
  2. European Commission. (n.d.-a). Controlling wear and surface cleanliness during cold rolling, LOWWEAR, RFSR-CT-2006-00010. CORDIS. Retrieved November 2026. https://cordis.europa.eu/project/id/RFSR-CT-2006-00010
  3. European Commission. (n.d.-b). Selective surface oxidation of the alloying elements in steels during recrystallization annealing, 7210-KB-210. CORDIS. Retrieved November 2026. https://cordis.europa.eu/project/id/7210-KB-210/results
  4. Inagaki, S., Ishii, T., Hu, Q., Ren, X. P., & Wakimoto, M. (2017). Development of rolling oil with cationic emulsifier for sheet gauge cold rolling. Tetsu-to-Hagane, 103(3), 134–141. https://doi.org/10.2355/tetsutohagane.TETSU-2016-055
  5. Kimura, Y., Fujita, N., & Mihara, Y. (2009). Plate-out behaviors of O/W emulsions for cold rolling in a short time interval. Tetsu-to-Hagane, 95(4), 340–346. https://doi.org/10.2355/tetsutohagane.95.340
  6. Komai, M., Fukuyama, S., Sato, T., & Iketaka, S. (1981). Formation of smudges and iron oxide film in the course of cold rolling. Tetsu-to-Hagane, 67(10), 1763–1769. https://doi.org/10.2355/tetsutohagane1955.67.10_1763
  7. Lee, J.-L. (2018). A study on carbonization on the surface of steel sheet during the BAF annealing process. Journal of the Korea Academia-Industrial cooperation Society, 19(7), 42–49. https://doi.org/10.5762/KAIS.2018.19.7.42
  8. Mogwaneng, P. J. (2008). Optimization of rolling mill oils evaluation using FT-IR spectroscopy [Master's dissertation, University of Pretoria]. https://repository.up.ac.za/handle/2263/27225
  9. National Fire Protection Association [NFPA]. (2023). NFPA 86, Standard for ovens and furnaces.
  10. Pillar, R., Ginic-Markovic, M., Clarke, S., Gibson, A., Bell, W., Brown, H., Willis, D., Renshaw, W., & Matisons, J. (2005). The effect of gas environment on rolling oil removal from cold-rolled steel as studied by TG. Journal of Thermal Analysis and Calorimetry, 80(1), 211–216. https://doi.org/10.1007/s10973-005-0638-1
  11. Sech, J. M., & Kleksiak, T. P. (1996). The evaluation of rolling oils used in the cold rolling of sheet steel by thermogravimetry. In Proceedings of the 33rd Rolling Seminar (pp. 325–340). ABM. https://doi.org/10.5151/2594-5297-LA5749
  12. U.S. Environmental Protection Agency [EPA]. (2002). Development document for final effluent limitations guidelines and standards for the iron and steel manufacturing point source category (EPA-821-R-02-004). https://www.epa.gov/sites/default/files/2015-10/documents/ironsteel_dd_2002.pdf
  13. Wang, D.-M., Inagaki, S., & Shiota, R. (2025). Factors affecting generation of iron fines in cold sheet rolling of steel. ISIJ International, 65(9), 1331–1338. https://doi.org/10.2355/isijinternational.ISIJINT-2025-124
  14. Wilson, P. R., Chen, Z., Killmore, C. R., Laird, S. J., & Williams, J. G. (2007). Surface oxidation of low carbon steel strip during batch annealing. ISIJ International, 47(1), 114–121. https://doi.org/10.2355/isijinternational.47.114

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.