Why do aluminium parts corrode white in storage?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Corrosion Prevention

Treating aluminium as a metal that does not rust, stacking bare parts as they are and wiping off white stains is the usual response, but the white powder is corrosion product formed where the oxide film broke down on a wet surface, so it comes back unless the conditions that wet the metal change. What actually lies behind it can be alkali and chloride left from cleaning, condensation, contact with wood, cardboard or other metals, water trapped in stacks, or a rust preventive unsuited to aluminium, and sometimes two or more at once.

Background

Open a box of aluminium housings taken out of storage and white blotches have spread across the surface here and there; scratch one with a fingernail and white powder comes away. Even after wiping, the spot stays dull, so parts due for painting, anodising or bonding have to be reworked or sorted out. Such stains have little effect on strength but look bad, and they can cause processing problems when further finishing or fabrication follows (Aluminum Association, 2009). For parts about to ship, the time spent sorting and reworking and the delayed delivery are lost as well.

Aluminium forms a thin oxide film the moment it meets air, and this film covers and protects the metal. The film is stable in water between roughly pH 4 and 9 and dissolves in water more acidic or more alkaline than that (Vargel, 2020). Equilibrium diagrams drawn against potential and pH show aluminium going into solution as aluminium ions on the acid side and as aluminate ions on the alkaline side (Pourbaix, 1974). A thin layer of water forms on aluminium surfaces in air, and acid and chloride dissolved in it either dissolve the oxide or take the place of its hydroxide, building up corrosion product. The white powder seen in storage is this kind of product, based on aluminium hydroxide (Graedel, 1989).

So tracing white corrosion back comes down to two questions: where the water came from and how long it stayed, and what was in it that broke the oxide film. Even in the same warehouse and the same season, cleaning, packing, supports and stacking give different answers to both.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: photograph where on the part the stains formed and what shape they take, note the part's cleaning record, storage place and time, packing, supports and the rust preventive applied, and compare them with the preventive's technical data sheet, the TDS.

Hypothesis 1: cleaning residue

Where machined parts go through an alkaline washer, rinse and dryer and are packed straight away, start with this hypothesis. It applies when cleaner keeps carrying over into the rinse tank and tips the rinse water to the alkaline side, when the rinse uses process water containing chloride, and when cleaner pools in blind holes or grooves and dries there. Suppose that on a Friday afternoon die-cast housings fresh from the washer, still warm, were wrapped in film and boxed. On Monday the box is opened, and white rims run around the tapped holes and along the tracks where water ran off.

An alkaline cleaner lifts oil and also dissolves a little of the oxide film on aluminium. If rinsing falls short, alkali stays on the surface and in crevices, and as the water dries what is left becomes more concentrated. When moisture or condensation inside the pack wets that spot again, the local pH moves beyond the range the oxide film can bear, the film dissolves, and the bared aluminium reacts with water to build up white hydroxide (Vargel, 2020). Chloride reaches the same result another way. Chloride ions break through weak points in the oxide film and start small pits, pitting corrosion, and inside a pit the dissolved metal ions react with water and turn it acidic, so the pit keeps itself growing (Frankel, 1998). Chloride carried in rinse water gathers in the marks left as water dries, so stains can follow the places where water ran and pooled.

Begin by measuring pH in the rinse water and on the surface. Measure pH and conductivity in the final rinse tank, and press a pH strip against the wet face of a part just out of the washer. If the rinse water has drifted from neutral or its conductivity is well above that of fresh water, cleaner may be carrying over. Check too whether stains cluster where liquid pooled and dried: around holes, at the bottom of grooves, on lower edges. Rinse some parts from one lot again in clean water straight after washing, dry them fully, and store them beside the rest; the comparison shows the difference.

If leftover cleaner is the cause, redesign the rinse. Run the rinse tank on overflow or change it at fixed intervals to keep pH and conductivity within limits, and make the final rinse with low-chloride deionised water. Blow out blind holes and grooves with compressed air, and after drying let parts cool to room temperature before packing. Check against the TDS that the cleaner is run at the supplier's concentration and temperature and that it is suitable for aluminium.

Hypothesis 2: condensation

Suspect condensation when day and night temperatures swing widely, as they do between seasons, when metal brought from a cold truck or an outdoor store is unpacked somewhere warm, and when warehouse doors stay open through night and day. Goods kept near walls, doors and windows cool down more easily. Picture a winter morning when bundles of sheet from a truck that drove through the night are moved straight into a heated workshop. Droplets soon form on the outside of the wrapping, and when the sheets are unpacked a few days later, greyish-white patterns have spread inwards from their edges.

Air always carries invisible water vapour, and the warmer it is, the more it holds. When the metal falls below the dew point of the surrounding air, the temperature at which vapour starts to turn into water, water forms on its surface. That happens when cold metal is moved somewhere warm and humid, or when metal cooled overnight cannot keep up with humidity that rises quickly during the day. Water that forms at the edges of stacked sheet or coils can be drawn in between them by capillary action (Aluminum Association, 2009). Even without visible droplets, the water layer on a surface thickens as relative humidity rises, and contamination that attracts water, such as dust or salt, lets a water layer form at lower humidity (Leygraf et al., 2016). That is why the standard that rates atmospheric corrosivity weighs how long surfaces stay wet together with pollutants such as chloride and sulphur dioxide (ISO, 2012).

A thermometer and a hygrometer are all the check needs. Work out the dew point from the temperature and relative humidity of the store, and compare it with the surface temperature of incoming metal or of parts inside the pack, measured with a contact thermometer. Metal colder than the dew point is in condensing conditions. A temperature and humidity logger left in the warehouse and inside shipments for a few weeks shows when condensation occurs, and moisture indicator labels that change colour or shape when wetted can be placed inside packs (Aluminum Association, 2009). If stains spread inwards from the edges of a bundle, or cluster on goods kept near walls and doors, lean towards condensation.

Once it narrows to condensation, work at keeping the metal above the dew point. Keep warehouse doors shut, keep goods away from walls and doors, and do not store them outdoors even when packed. Let cold metal warm up slowly in its unopened pack somewhere free of draughts before bringing it into the workshop, use vehicles with intact covers, and avoid long layovers on the way. If it is already wet, the guidance is to use it at once and dry it as it is used, or to unpack it and dry it with moving air (Aluminum Association, 2009).

Hypothesis 3: contact materials

If stains appear only where supports or packaging touched, look at the material in contact. Cases include under-dried wooden pallets or bearers, damp cardboard boxes and dividers, and storage against steel racks, copper parts or stainless fixings. A typical scene: aluminium extrusions left for a few weeks on timber bearers in a warehouse during the rainy season. When the bearers are removed, white bands as wide as the bearers cross the underside, and the parts that did not touch are sound.

Wood holds water. Its moisture content rises and falls with the surrounding humidity, and metal embedded in or touching wood starts to corrode once moisture content passes 15 to 18%, corroding faster the higher it goes. The same review notes that copper-based wood preservatives increase corrosion of the metals they touch (Zelinka, 2014). Wood also gives off organic acid vapours such as acetic and formic acid (Gibson & Watt, 2010). Yet when acid vapours from wood were tested against many metals, steel, zinc and magnesium were attacked while aluminium held up comparatively well, so for aluminium the first thing to look at is wet wood holding water against the surface rather than the acid vapour (Clarke & Longhurst, 1961). Cardboard and paper also hold water against the faces they touch once they take up moisture.

Contact with other metals becomes a problem when water is present. Where two dissimilar metals touch and water bridges them, a small cell forms, and paired with copper, stainless steel or steel, aluminium is usually the side that dissolves. A US Department of Defense standard rates whether metal pairs are compatible by the corrosion rate calculated from the current flowing between them, and calls for protection where an incompatible pair has to be in contact (DoD, 2021). So the same rack may do no harm on dry days, yet once condensation or wet packaging supplies water, corrosion starts at the points of contact.

Measure the condition of supports and packaging first. Check the moisture content of pallets and bearers with a wood moisture meter, and feel whether the cardboard is damp. Lay the shape of the stains over the positions of bearers, dividers and racks; if they match the contact marks, this hypothesis is strong. Where metal touched, note the other metal and whether water could have collected between them, and for wood, ask the supplier whether it was preservative-treated.

The fix is to break the link between aluminium and any material that can get wet. Switch supports to well-dried timber or plastic, and keep preservative-treated wood from touching aluminium directly. Put plastic film or a corrosion-inhibiting interleaf between cardboard and aluminium, and separate racks and fixings of other metals with insulating pads. Set a moisture content limit for timber supports and accept deliveries against it.

Hypothesis 4: trapped water

This hypothesis applies when sheet, extrusions or machined parts are stacked tight or wound into coils, and when parts are packed face to face. The faces in contact cannot be seen from outside and come to light only when pieces are lifted off one by one for use. An example: a bundle of sheet stored for nearly two months, the top few sheets clean, but further down, map-like greyish-white patterns spreading wider between one sheet and the next.

Water that gets between faces in contact has no way to dry. When water sits for a long time in a gap with no air flow, it reacts with the metal and leaves a stain, and the guidance explains these stains as water trapped between the wraps of a coil or between stacked sheets (Aluminum Association, 2009). The thin water in the gap hardly exchanges with the outside air or water, so what dissolves from the oxide film and any salt carried in build up there. Where flat faces overlap over a wide area, the reaction spreads into patterned stains, and given time the surface is roughened (Vargel, 2020). The trapped water may come from condensation, or from parts stacked before they were fully dry after cleaning.

Unpack the bundle, turn the pieces over one by one and note where the stains are. If they spread wider on the faces in contact than on the outer faces, and wider in the middle of the contact than at the edges, suspect trapped water. If there was interleaving paper, see whether it got wet or carries water marks. Look up the part temperature and dryness just before stacking in the records, and compare how staining varies with stack height and storage time.

To cut down trapped water, close the gaps it gets into or give water that gets in a way to dry. Stack surface-critical sheet with interleaving, and stack washed or wet parts only once they are fully dry. A bundle that has already taken in water should be opened at once, spread out and dried with moving air, warm air if possible, as the guidance describes (Aluminum Association, 2009). For goods held a long time, lower the stack height and use the oldest stock first.

Hypothesis 5: unsuitable preventive

This hypothesis comes up where the rust preventive oil or water-based preventive used on steel parts goes onto aluminium parts unchanged. The same holds right after a change of preventive, after the dilution of a water-mixed product changes, and where aluminium and steel run through one line together. One can picture steel parts kept the same way in the same warehouse staying clean, while white spots break out only on the aluminium parts that were treated and put away.

Rust preventives are formulated for the metal they protect. If what stays in the film is alkaline, then when moisture or condensation wets it, the water on the surface can move beyond the pH range the oxide film can bear, and the product then dissolves the film instead of protecting it (Vargel, 2020). The classification standard for temporary corrosion protection lists uses for each product category, and aluminium sheet appears among the examples for categories such as solvent-applied oily films, waxy films and peelable films (ISO, 1987). Aluminium producers, too, want to confirm that a water stain preventive suits the customer's process before applying it, and on request apply synthetic oils that contain no water (Aluminum Association, 2009). When condensation lands on an unsuitable preventive, white corrosion can start right there.

Look first in the preventive's TDS and safety data sheet, the SDS, for the metals it suits, its pH and its dilution. For a water-mixed product, measure the pH at working strength, and put a drop of distilled water on a treated part and read it with a pH strip. Split aluminium coupons from one lot into untreated, treated with this preventive, and treated with another, keep them side by side under condensing conditions and compare; that separates the preventive's share.

If the preventive proves unsuitable, change to a product stated to be suitable for aluminium, or use different products on aluminium and steel. Keep water-mixed products at the supplier's dilution, and confirm the effect with coupon comparisons before switching. Where the metal is bought in, agree in advance with the producer on the type of oil film applied at dispatch.

Finding the cause

Five hypotheses do not mean five separate investigations. Rule them out one at a time, starting with what is easy to measure. pH strips, a temperature and humidity meter and a wood moisture meter give answers within a day, and the cleaning, receiving and storage records are already at hand. Coupon comparisons take weeks, so they come after.

The biggest clue is where the stains are and what they look like. Stains along holes or the tracks of running water point to alkali and chloride left from cleaning; stains spreading inwards from the edges of a bundle, or clustering on goods near walls and doors, point to condensation. Stains that match the positions of bearers, dividers or racks point to contact materials, and stains spread widely inside the faces in contact while the outer faces are clean point to trapped water. If steel parts under the same conditions are fine and only treated aluminium is stained, look at the preventive first.

When it appeared also divides the paths. A rise a few days after cold deliveries were unpacked, or a sudden increase as the seasons change, points to condensation; stains only in lots packed straight after washing point to cleaning residue. If staining worsens the longer goods stay stacked or sit on supports, trapped water or contact materials are the stronger candidates.

If that still does not settle it, run control trials. Split parts from one lot and change one thing for one group only: rinse and dry them again, add interleaving, switch the supports to plastic, or change the preventive, then keep both groups in the same place. Change only one thing at a time, or there is no telling which one worked. Afterwards, count stained parts per lot on the same basis as before the change, and the job is done only when that figure has recovered.

The hypotheses often act together. Condensation supplies water to the others, cleaning residue adds alkali and chloride to that water, and tight stacks and wet supports hold it in place for a long time. In such cases cut off the water first. Keep the metal above the dew point and stack it only when fully dry, then look at cleaning and the preventive again, because while water keeps getting in, the effect of changing anything else cannot be compared fairly.

Limits and cautions

Cleaner concentration, rinse limits, and the metals and dilution a preventive suits differ by product, so numeric decisions follow the product's TDS and the supplier's guidance. Corrosion looks different on different alloys and finishes, so review anodised or conversion-coated parts together with the finisher. Where white corrosion has dug deep, or for safety-related parts such as aerospace, pressure vessel or structural components, do not decide on use from appearance alone; get tests such as cross-section examination and the quality engineer's judgement.

Safety matters too. For alkaline cleaners and preventives, follow the SDS for gloves, eye protection and ventilation. Keep dust down when brushing or grinding off white powder, and follow forklift and lifting procedures when opening and restacking heavy bundles. Do not use old mercury thermometers to measure metal temperature, because mercury from a broken one can corrode aluminium (Aluminum Association, 2009).

Sources

  1. Aluminum Association. (2009). Guidelines for minimizing water staining of aluminum (TR3, 5th ed.). https://www.aluminum.org/sites/default/files/2021-11/WaterStainingGuidelines.pdf
  2. Clarke, S. G., & Longhurst, E. E. (1961). The corrosion of metals by acid vapours from wood. Journal of Applied Chemistry, 11(11), 435–443.
  3. Frankel, G. S. (1998). Pitting corrosion of metals: A review of the critical factors. Journal of the Electrochemical Society, 145(6), 2186–2198. https://doi.org/10.1149/1.1838615
  4. Gibson, L. T., & Watt, C. M. (2010). Acetic and formic acids emitted from wood samples and their effect on selected materials in museum environments. Corrosion Science, 52(1), 172–178. https://doi.org/10.1016/j.corsci.2009.08.054
  5. Graedel, T. E. (1989). Corrosion mechanisms for aluminum exposed to the atmosphere. Journal of the Electrochemical Society, 136(4), 204C–212C.
  6. International Organization for Standardization [ISO]. (1987). ISO 6743-8:1987, Lubricants, industrial oils and related products (class L) — Classification — Part 8: Family R (Temporary protection against corrosion). https://www.iso.org/standard/13217.html
  7. International Organization for Standardization [ISO]. (2012). ISO 9223:2012, Corrosion of metals and alloys — Corrosivity of atmospheres — Classification, determination and estimation.
  8. Leygraf, C., Odnevall Wallinder, I., Tidblad, J., & Graedel, T. (2016). Atmospheric corrosion (2nd ed.). Wiley.
  9. Pourbaix, M. (1974). Atlas of electrochemical equilibria in aqueous solutions (2nd English ed.). NACE.
  10. U.S. Department of Defense [DoD]. (2021). MIL-STD-889D, Galvanic compatibility of electrically conductive materials.
  11. Vargel, C. (2020). Corrosion of aluminium (2nd ed.). Elsevier.
  12. Zelinka, S. L. (2014). Corrosion of metals in wood products. In M. Aliofkhazraei (Ed.), Developments in corrosion protection. InTech. https://doi.org/10.5772/57296

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.