Blaming the preventive and changing products is the usual response when only flanges rust first, but if the body coated with the same product on the same day is sound, the trouble more likely lies in the flange as a location rather than the product, so a change of product alone tends to see rust return to the same spots. What actually lies behind it can be a film thinned at edges, water in bolt holes and threads, missing or gapped protective caps, gasket faces damaged in handling or porosity in cast surfaces, and sometimes two or more at once.

Background

Flanged parts such as valves, pumps, pressure vessel nozzles and pipe spools go into storage or out for shipment, and while the body and broad faces stay sound, rust comes up first only on the flange: the gasket face, the outer edges, and inside and around the bolt holes. Rust and marks on a gasket face can spoil the seal, so the face has to be remachined or judged for replacement, and installation slips by that much. Rust in threads gets in the way of fitting and tightening bolts.

If, among parts coated with the same preventive on the same day, rust reaches the flanges first, those spots are where the film is thin, where water stays long, or where the film has been damaged. Atmospheric corrosion is set by the time a surface stays wet together with airborne pollutants, so rust gets ahead wherever water lingers (ISO, 2012). The design standard for protective paint systems likewise treats sharp edges, narrow gaps and blind crevices, and bolted connections as weak points for corrosion protection in their own right (ISO, 2017a).

A flange is where these weak points gather in one place. Sharp machined edges, bolt holes and threads, the face a cover touches, and a precisely machined gasket face of bare metal all sit within a hand's width, and on a casting there is also porosity opened up by machining. The broad faces of the body have few such spots, which is why the same preventive looks ample there. So where on the flange the rust started, and in what shape, narrows the cause sharply.

For this symptom the technical team sets up the five hypotheses below and works through them in turn. The first task is the same every time: photograph the rusted flanges, note whether the rust started at edges, inside holes, at cover marks, along scratches or as small dots, and compare the preventive type and how it was applied, the type and fit of covers, and the storage location with the preventive's technical data sheet, the TDS.

Hypothesis 1: thin film at edges

Look at this hypothesis for flanges given a single thin coat by brush or spray, for sharp edges left undressed after machining, and for the sharp rims at the mouths of bolt holes. It applies especially when rust runs as a fine line along the inner edge of the gasket face, round the outer rim of the flange or round the mouths of bolt holes. Envisage pipe spools sprayed with preventive oil before shipment and laid on a rack in the yard. A few weeks later the broad faces are still oily, but a fine line of rust rings the outer rim of each flange and the mouth of every bolt hole.

A liquid film thins at edges on its own. Where curvature changes abruptly, as at edges and the rims of holes, surface tension sets up pressure differences, and the sharper the edge, the greater the pressure that drives the liquid away, leaving the film very thin (Eley & Schwartz, 2002). Preventives are usually designed to go on as a single coat 2 to 20 µm thick (McGuire, 2016), so a film that is ample on a flat face may leave almost nothing on an edge. That is also why the paint system design standard recommends rounding or chamfering sharp edges (ISO, 2017a).

Check first whether the rust follows the edges as a line. Use a magnifier to see whether burrs remain and how sharp the edges are, and just after rust prevention press oil-absorbing paper against an edge and a flat face with the same force to compare how dark the marks are. With spray application, look too at the angle at which the nozzle passes edges and hole mouths. Check as well whether a chamfer is applied in machining and whether the drawing calls for one.

If edges are the cause, deal with the edges themselves and with how the preventive goes on. Remove burrs and add a small chamfer in machining, and give edges and bolt-hole mouths a second coat by brush. For parts going into long storage, review a grade that dries to a firm or thicker film, and protect flange faces with covers as well. On a spray line, one nozzle can be turned to aim separately at edges and hole mouths.

Hypothesis 2: water in bolt holes

When flanges lie face-up or stand without a roof over them, rain, dew and wash water collect in bolt holes and tapped holes. It is worse with blind tapped holes, such as the stud holes of valve bodies, and with through holes whose lower end is closed off by a support. A familiar yard sight: pump casings stood on pallets with the suction flange facing up. The day after the rain stops, every tapped hole is full of water, and later rings of rusty water spread round the hole mouths.

Narrow gaps and blind crevices hold moisture, dirt and soluble salts, which makes them especially prone to corrosion (ISO, 2017a). Liquid can enter a small hole closed at one end only as the air inside gets out (Matsumoto et al., 2022), so preventive brushed or sprayed on briefly may well not reach the bottom of a tapped hole. An upward-facing hole, by contrast, takes in water every time it rains and slowly fills. Once in, water dries far more slowly than on the outside, and since the bottom of the hole and the thread roots get less oxygen than the mouth, a small cell forms in which the oxygen-poor inside becomes the side that dissolves (Revie & Uhlig, 2008).

Check storage position and exposure to rain first. Put a thin swab into the holes to see whether water and preventive are there, and see whether rust sits at the bottom, in the thread roots or as a ring round the mouth. Comparing holes plugged and left open on the same part shows how much water accounts for. For yard storage, match the days it rained with the day rust was first seen, using weather records.

If water is the cause, remove both its way in and the places it can stay. Store flanges so faces do not point upwards, or under a roof, and close tapped holes with plugs or preventive plugs. Blow out and dry holes that are already wet before coating them again, and inject preventive to the bottom of tapped holes with a fine nozzle. Review with the supplier whether a water-displacing preventive suits.

Hypothesis 3: absent or loose caps

Look at this hypothesis when covers have come off in transit, when they were removed for inspection or measurement and not put back, when plastic caps are the wrong size or have perished and cracked in the sun, or when a cardboard cover held by a single strip of tape has got wet and lifted. It weighs more if rust is only on uncovered flanges, or follows the rim of a cover's outline. Here is how it can look when a bundle of pipe spools is unpacked on a construction site. Some flanges lost their covers on the way, some remaining covers have lifted at the edges, and the rust follows the uncovered faces and the rims under the lifted covers.

A cover is a wall that keeps rain, dust and hands off the face, and when a volatile corrosion inhibitor is used, it is the lid that makes a closed space. A US military standard for storing industrial plant equipment likewise called for pipe ends to be closed with plugs or caps and very large openings to be covered with wood or sheet material (DoD, 2001). A volatile inhibitor protects by spreading as vapour through a closed space and clinging to the metal, so a cover with gaps keeps it from reaching the concentration it needs (Gangopadhyay & Mahanwar, 2018). A gapped cover can even catch rain and hold water in the narrow gap between face and cover, and as the face under it warms by day and cools by night its temperature can fall close to the dew point so that water condenses (ISO, 2017b).

Compare rust on flanges that had covers with rust on those that did not, side by side. Remove the remaining covers to see whether there is water or condensation marks inside, whether the size and material suit the flange, and whether they have cracked or perished. Check in the transport, inspection and measurement records who removed covers and when.

If covers are the cause, specify both the covers and the procedure for handling them. Choose covers sized to cover the whole gasket face and either bolted on or a tight fit, and seal their edges with waterproof tape. Make re-coating and refitting part of the procedure whenever covers come off for inspection, and if a volatile inhibitor goes inside, make sure the cover closes completely. Mark parts whose covers have been off and refitted, so the next inspection looks at those flanges first.

Hypothesis 4: damaged gasket face

Look at this hypothesis when flange faces are dragged along the floor, stacked face to face, or touched by lifting hooks or chains, and when faces are rubbed with bare hands or tools during inspection. It applies especially when rust follows scratches, dents or fingerprints on the gasket face. One example: several valves stacked face to face on a pallet slide against one another while a forklift moves them. At the shipping inspection a few fine lines show on the gasket faces, and the rust follows those lines.

A preventive film is thin, and as temporary protection it is easily damaged (McGuire, 2016). The moment it is scratched, that spot is bare metal, and the groove of the mark holds moisture and dirt. Bare-hand prints bring rust by another route. Sweat contains salts such as sodium chloride, so a touch leaves salts behind that draw in moisture (Cadd et al., 2015). Marks on a gasket face are not only a rust problem. Guidance on bolted flange joint assembly assesses damage to a gasket face by how far it extends across the width the gasket seats on and by its depth, with different allowances for different gasket types (ASME, 2022).

Use a magnifier to see whether the rust follows marks as lines or dots. Whether bright metal remains at the bottom of a mark, and which came first, the mark or the rust, tells whether it is handling damage. Then follow the flange along its route after machining, through stacking, transport and inspection, and see what the face touches. Record the direction, length and depth of marks, and leave the judgement on whether the face can still seal to the quality engineer.

If handling is the cause, make sure the face touches nothing. Move flanges with a support under the face or with covers fitted, do not stack them face to face, and attach hooks and chains where they cannot reach the face. Wear gloves for inspection, and coat faces again once inspection is done. Fit dividers in shipping crates too, so faces cannot touch. Judge existing marks separately from removing the rust.

Hypothesis 5: casting porosity

Look at this hypothesis when machining the flange face of a cast steel or cast iron valve body or pump casing has opened up porosity beneath the surface. It weighs more when rust appears as scattered small dots on the gasket face, and rusty liquid seeps from them some time after washing. A few days after a cast valve body's flange face has been machined, washed and coated, brown dots like pinpricks appear scattered across the gasket face. Some of them come back wet even after being wiped.

Castings can retain shrinkage porosity, formed as the metal contracts on solidifying, or gas porosity, formed where gas was trapped (Campbell, 2015). Machining opens these pores at the face, and narrow holes draw in coolant or cleaner by capillary action, to a depth that grows with time (Washburn, 1921). Liquid in the pores dries far more slowly than the outside, seeps back out under the preventive film and keeps the metal round the pore wet. Impregnation, filling the pores with resin, is a process for which a US military standard sets out requirements and tests for nonferrous castings (DoD, 1992).

Use a magnifier to see whether each rust dot has a small hole at its centre. Leave washed parts somewhere warm to see whether liquid seeps from the dots, and comparing dot counts between casting lots shows how much porosity accounts for. Whether porosity on the gasket face matters for sealing is judged separately from the rust, against joint assembly guidance and design criteria.

If porosity is the cause, add a step that dries the pores out. After washing, blow the face with compressed air and draw liquid out of the pores with warm air or vacuum drying before coating, and choose on test pieces a grade that leaves a film able to bridge the pores. Leaving parts somewhere warm for a while before coating, then wiping off what seeps out and drying again, also helps. If sealing faces show a lot of porosity, review with the foundry, separately from the rust, whether impregnation can be used on that material and whether casting conditions can change.

Finding the cause

Of the five hypotheses, the first to be ruled out are the ones the eye can see. Whether covers were fitted, which way flanges faced and whether they got rained on can be confirmed at the storage location straight away. Edge condition, marks and porosity need only a magnifier, and test-piece comparisons and sections come after that.

The shape of the rust is the best clue. Fine lines along edges and hole mouths point to film thinned at edges, and rust at the bottom of holes, in thread roots or as rings of rusty water round the mouth points to standing water. Rust on faces that had no cover, or along the rim of a cover's outline, points to covers and caps; rust that follows scratches and fingerprints points to handling damage; and scattered small dots with a hole at their centre point to casting porosity.

If the shape does not settle it, split flanges from one lot for control trials. Change one thing per pair, edges given a second coat against edges left as they are, holes plugged against holes left open, tight-fitting covers against the current covers, and keep them in the same place. Change two things at once and there is no telling which one stopped the rust.

The final check is to send real parts treated by the corrected method through real storage and transport, then examine the flanges again. Photograph edges, hole interiors, the area under covers and the gasket face at the same spots recorded at the start, and compare. If rust does return, whether it comes back at the same spots or moves elsewhere shows which cause remains.

Two causes can also arrive together. A lifted cover channels rain into the bolt holes, and a film already thin at the edges exposes bare metal at the slightest scratch in transport. In such cases first put right the routes by which water gets in and stays, namely covers and storage position, and then look at edges, handling and porosity, because while water keeps coming and going, the effect of changing the preventive or how it goes on cannot be compared fairly.

Limits and cautions

Preventive grade and film thickness, edge treatment and cover specifications differ with the part, storage time, transport route and customer specification, so numeric decisions follow the preventive's TDS and the supplier's and customer's requirements. Whether rust, marks or porosity on a gasket face can be accepted is judged by the quality engineer against joint assembly guidance and design criteria, and pressure equipment is never released on floor judgement alone. Before removing rust from a gasket face by polishing, check first that the flatness and finish requirements for the face will still be met.

Safety matters too. Follow each preventive's and cleaner's safety data sheet, the SDS, for gloves, eye protection and ventilation. Use lifting equipment when turning heavy flanged parts or fitting and removing covers so hands are not trapped, and wear eye protection against water and chips when blowing out bolt holes with compressed air.

Sources

  1. American Society of Mechanical Engineers [ASME]. (2022). ASME PCC-1–2022, Pressure boundary bolted flange joint assembly.
  2. Cadd, S., Islam, M., Manson, P., & Bleay, S. (2015). Fingerprint composition and aging: A literature review. Science & Justice, 55(4), 219–238. https://doi.org/10.1016/j.scijus.2015.02.004
  3. Campbell, J. (2015). Complete casting handbook: Metal casting processes, metallurgy, techniques and design (2nd ed.). Butterworth-Heinemann.
  4. Eley, R. R., & Schwartz, L. W. (2002). Interaction of rheology, geometry, and process in coating flow. Journal of Coatings Technology, 74(932), 43–53. https://www.paint.org/wp-content/uploads/2021/09/jctSEPT02-Eley.pdf
  5. Gangopadhyay, S., & Mahanwar, P. A. (2018). Recent developments in the volatile corrosion inhibitor (VCI) coatings for metal: A review. Journal of Coatings Technology and Research, 15(4), 789–807. https://doi.org/10.1007/s11998-017-0015-6
  6. International Organization for Standardization [ISO]. (2012). ISO 9223:2012, Corrosion of metals and alloys — Corrosivity of atmospheres — Classification, determination and estimation. https://www.iso.org/standard/53499.html
  7. International Organization for Standardization [ISO]. (2017a). ISO 12944-3:2017, Paints and varnishes — Corrosion protection of steel structures by protective paint systems — Part 3: Design considerations.
  8. International Organization for Standardization [ISO]. (2017b). ISO 8502-4:2017, Preparation of steel substrates before application of paints and related products — Tests for the assessment of surface cleanliness — Part 4: Guidance on the estimation of the probability of condensation prior to paint application.
  9. Matsumoto, Y., Mizushima, Y., & Sanada, T. (2022). Removing gas from a closed-end small hole by irradiating acoustic waves with two frequencies. Micromachines, 13(1), 109. https://doi.org/10.3390/mi13010109
  10. McGuire, N. (2016, September). Fundamentals of rust preventives used for temporary corrosion protection. Tribology & Lubrication Technology, 28–34. https://www.stle.org/images/pdf/STLE_ORG/BOK/LS/Metalworking/Fundamentals%20of%20RUST%20PREVENTIVES%20used%20for%20temporary%20corrosion%20protection.pdf
  11. Revie, R. W., & Uhlig, H. H. (2008). Corrosion and corrosion control: An introduction to corrosion science and engineering (4th ed.). Wiley. https://doi.org/10.1002/9780470277270
  12. U.S. Department of Defense [DoD]. (1992). MIL-STD-276A, Impregnation of porous nonferrous metal castings. https://everyspec.com/MIL-STD/MIL-STD-0100-0299/MIL-STD-276A_17046/
  13. U.S. Department of Defense [DoD]. (2001). MIL-STD-107J, Preparation and handling of industrial plant equipment (IPE) for shipment and storage. Cancelled without replacement 2010. https://everyspec.com/MIL-STD/MIL-STD-0100-0299/MIL-STD-107J_20749/
  14. Washburn, E. W. (1921). The dynamics of capillary flow. Physical Review, 17(3), 273–283. https://doi.org/10.1103/PhysRev.17.273

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.