Raising the coolant concentration is the usual response to rust between operations, but rust can start anywhere after the part leaves the machine, in washing, rust prevention, stacking or waiting, so fixing concentration alone often lets it return. What actually lies behind it can be salts and a thin film left by dried coolant, protection stripped in washing, a diluted and contaminated in-process preventive, water trapped between stacked parts or a wait longer than the protection lasts, and sometimes two or more at once.

Background

A part fresh off the machining centre goes onto a waiting rack in front of the next operation. While it waits its turn for heat treatment, grinding, plating or assembly, red spots appear on the machined faces and dark stains spread where parts lie on top of one another. Rust has to be wiped off or machined away, and precision faces can fall out of size or finish and be scrapped. If a rusted part moves on to the next operation, plating adhesion and heat-treatment quality can suffer too.

Rust on steel grows where a thin film of water sits on the surface with oxygen and ions dissolved in it. Iron dissolves into the film, the freed electrons are used where oxygen meets water to form hydroxide ions, and the two meet to form rust (Revie & Uhlig, 2008). That is why the international standard that classifies atmospheric corrosivity treats time of wetness, the time the surface stays wet, together with airborne pollutants as the key factors (ISO, 2012).

During machining, the corrosion inhibitors dissolved in a water-miscible coolant protect the metal, and coolant residue left on the part can give a few weeks of protection as well. A rust preventive, by contrast, is a film applied separately once machining is done (McGuire, 2016). Rust between operations usually forms in the gap between where the coolant's protection ends and the next protection begins. That gap can come from the coolant itself, from the washing or rust prevention step, or from how and how long the parts are kept.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: collect rusted and sound parts together, photograph where the rust began, and log the waiting time from the end of machining to the first sight of rust, the temperature and humidity in that time, and the concentrations of the coolant and the in-process preventive, then compare them with each product's technical data sheet, the TDS.

Hypothesis 1: weak coolant residue

Look first at lines where parts go straight to the waiting rack still wet with coolant and unwashed. This hypothesis gains weight when the coolant concentration has fallen below its control range, when the make-up water is hard or salty, and when chips and fines dry onto the surface. Picture shafts machined in the afternoon, given a quick blow with compressed air and stood on a pallet. Next morning, every spot where the coolant dried carries a thin white rim, with brown dots lined up along it.

Coolant left on a part grows stronger as its water evaporates, until the inhibitor and the salts that were dissolved in the water are left on the surface. With enough inhibitor this residue protects the metal for a while, but residue from a lean fluid carries that much less inhibitor. Inhibitors also cling to chip surfaces and leave the fluid that way, so the inhibitor alone can be depleted while the overall concentration looks right (Eppert et al., 2003). The salts left behind draw moisture from the air. Sodium chloride takes up water from the air and turns into a solution above about 75% relative humidity (Greenspan, 1977), and carbon steel loaded with acidified artificial seawater particles kept corroding even when relative humidity was lowered to 11% (Schindelholz et al., 2014).

Check first whether the rust started at the rims of dried marks or where chips had stuck. Measure the coolant concentration in the sump with a refractometer and compare it with the TDS range; because evaporation shifts concentration, measure at set intervals, and check the hardness and quality of the make-up water too (HSE, 2021). The fluid's rust protection can be seen with the standard test that wets grey cast iron chips with diluted fluid to find the weakest concentration that leaves no rust stain. Its results usually relate to rust on nested parts or in drilled holes containing chips (ASTM International, 2022).

If the residue has weakened, put the fluid right first. Bring concentration back within the TDS range by topping up with premixed fluid rather than pouring in neat concentrate, and agree make-up water quality with the supplier. Wash or blow chips and fines off right after machining so they do not dry on the surface. If waits are longer than the residue can hold out, stop relying on it and add a separate in-process rust prevention step.

Hypothesis 2: protection washed off

If an alkaline or water wash sits between machining and the next operation, suspect the washing step. Typical cases are a plain-water rinse with nothing after it, the period just after a change of cleaner, and a rise in temperature or concentration to improve degreasing. Say gear blanks come out of the washer before heat treatment and are left, still warm, in their baskets in the waiting area. Unwashed, these parts could stand for days, yet the washed baskets turn evenly brown by the next day, starting from the top faces.

Washing removes the oil and, with it, the inhibitor that the coolant residue had been providing. The residue's protection only holds while that film stays on the metal (McGuire, 2016). In an alkaline wash, iron sits in the region where a thin oxide film protects it, but a plain-water rinse brings the pH down towards neutral and that protection is lost (Pourbaix, 1974). In the last stage of drying the remaining water film is very thin, so oxygen has only a short way to reach the metal, and rust can grow faster than under immersion (Stratmann & Streckel, 1990).

Splitting one lot into washed and unwashed parts and keeping them side by side shows washing's share straight away. If rust appears only on washed parts, and evenly across wide faces, this hypothesis moves to the front. Measure the pH and inhibitor concentration of the final rinse tank, and see how long washed parts take to dry fully and whether water is left in holes and gaps.

If washed parts wait before the next operation, protection has to be put back. Add a water-based inhibitor to the final rinse, or add a step that applies rust-preventive oil after drying. For parts machined with water-miscible coolant, treat dewatering or drying as part of the protection (NPL, n.d.). Too little of an oxidising inhibitor can even cause local attack, so keep within the supplier's recommended range (Revie & Uhlig, 2008). If the next operation is plating or heat treatment, first test that the inhibitor does not interfere with it.

Hypothesis 3: diluted, dirty bath

On lines that dip or spray parts with a water-based or water-displacing preventive between operations, what matters is whether that preventive is still as it started. Trouble comes when wet parts go in without pause and water and coolant build up in the tank, when topping up is done by eye, and when the tank goes a long time without a change. Think of a preventive dip tank placed right after the washer. After weeks of wet baskets going in and out, the liquid is cloudier than at the start, chip dust lines the bottom, and although the product has not changed, only recently dipped parts rust while waiting.

Inhibitors cling to the metal surface and form a thin layer that keeps out water and oxygen, so if their concentration in the liquid falls short, that layer becomes patchy (Tang, 2019). In dip application, water carried in on the parts mixes with the preventive and can reduce its protection, and water-based preventives displace water poorly, with impurities such as hard-water minerals able to cause problems (McGuire, 2016). Coolant and cleaner that get in do more than dilute the inhibitor; they also bring salts and alkali with them. When an oxidising inhibitor runs short, rust can dig in as deep spots rather than spreading widely (Revie & Uhlig, 2008).

Measure the tank concentration with a refractometer or the supplier's method and compare it with fresh product. Stand a sample from the tank in a graduated cylinder to see whether water or oil separates out; the standard test for oil and water separation is a useful reference (ASTM International, 2021). A foul smell or cloudy colour can signal microbial growth in a water-diluted liquid (Passman & Küenzi, 2020). Finally, dip identical test pieces in fresh product and in tank liquid, keep them in the same humid place and compare how they rust.

If the tank liquid performs worse than fresh product, set control rules. Measure concentration at fixed intervals, top up with liquid mixed at the set ratio rather than with neat concentrate, drain off settled water and sludge, and fix a change interval. If wet parts go straight in, either shake off or dry them before dipping, or review a switch to a water-displacing preventive with the supplier.

Hypothesis 4: wet stacked parts

Where flat parts such as washers, rings and plates are stacked neatly, or small parts are tipped into baskets by the heap, the faces in contact need watching. It happens especially when parts are stacked before they are fully dry after washing, and when warm parts are left to cool in a stack. One such scene: ground rings threaded onto a bar and stacked. The outer faces are clean, but when each ring comes off at the next operation, the faces that touched carry round dark stains and rings of rust.

A very narrow gap between two flat faces in contact draws in moisture by capillary action and is slow to give it up, holding salts and dirt along with it (ISO, 2017a). Oxygen reaches the inside of the gap poorly while the outside has plenty, so a small cell forms in which the oxygen-poor inside becomes the side that dissolves (Revie & Uhlig, 2008). There is a separate test that stacks coated panels and heats them, also run with water mixed into the preventive, meant for places where air cannot get between the layers. Corrosion there shows as dark staining rather than red rust (McGuire, 2016).

Check whether the rust is only on faces that touched, in the exact shape of the contact. Find out how warm the parts were when stacked, and whether water was left in the gaps even though they looked dry. Keeping the same parts stacked and stood apart in the same place makes the share due to stacking clear.

If stacking is the cause, change how parts are kept so water cannot be trapped. Stack only once parts are dry right through and cooled to room temperature, put rust-preventive paper or interleaves between them, or move to racks that stand parts apart so faces do not touch. If stacking cannot be avoided, choose a preventive grade that stayed free of stains in the stacked-panel test.

Hypothesis 5: too long a wait

Consider this hypothesis when waits grow longer than usual because of weekends and holidays, breakdowns or a backed-up schedule at the next operation. It applies all the more in the rainy season and at the turn of the seasons, and on racks near doors, vents or the floor. Imagine flange blanks finished on a Friday that wait until the middle of the following week because the next machine has broken down. They normally move on within a day, so no rust prevention was applied, and it rained through that week.

Protection between operations holds only for a limited time. Coolant residue is protection for a few weeks, and a rust-preventive film for weeks to months (McGuire, 2016). That time depends heavily on the humidity of the air. In a classic study of the atmospheric corrosion of iron, the rate of rusting rose sharply once relative humidity passed a critical value, and pollutants such as sulphur dioxide and airborne particles raised it further (Vernon, 1935). When the temperature drops overnight, or cold parts meet warm, humid air, the surface temperature falls close to the dew point and water condenses; the risk is judged by comparing surface temperature with the dew point worked out from air temperature and relative humidity (ISO, 2017b).

Finding the waiting time of the rusted lot in the records and comparing it with the usual is the first step. Put a temperature and humidity logger in the waiting area to see the humidity and the swings in temperature over the period when rust appeared, and check whether rust clustered on racks near doors or vents. Preventives can be ranked against one another for endurance in a humidity cabinet, but the results are a screen for ranking only and do not predict real storage life (ASTM International, 2024).

If the rusted lots turn out to have waited longer than usual, set for each operation how long parts may wait without rust prevention, and send parts that will exceed it through in-process rust prevention or packing. Make sure a delay in the schedule triggers an alert for lots in waiting, and move parts on first in, first out. Keep the waiting area dry and away from doors and vents, and do not leave packs open when moving cold parts into a warm area.

Finding the cause

Five hypotheses do not mean five separate investigations. The quickest thing to look at is the records. Waiting time, temperature and humidity in the waiting area, and the concentrations of coolant and preventive are mostly already logged or can be measured within a day. Washing conditions and stacking practice can be confirmed with one walk round the floor, and comparisons with test pieces come after that.

The first clue is the shape of the rust. Dots lined up along the rims of dried marks or where chips sat point to coolant residue and salts, and an even change across the wide faces of washed parts points to protection stripped in washing. Rust that appeared only after the preventive tank had been in use a long time points to dilution and contamination of the preventive; dark stains in the shape of contact on faces that touched point to stacking; and rust only on lots that waited unusually long points to waiting time.

If the shape does not settle it, run control trials. Split one lot in two and change one thing at a time, washed against unwashed, fresh preventive against tank liquid, stacked against stood apart, keeping both halves in the same place. That way it is clear which change made the difference.

The final check after a fix is made with real parts. Keep parts from the corrected process in the same waiting area for a little longer than the longest usual wait and see that they stay free of rust. Checking once more in the humid season reduces the chance of rust returning when the season changes.

The hypotheses can overlap. Salts left by a lean coolant hold water in stacked gaps for longer, and parts stripped of protection in washing rust after even a slightly longer wait. In such cases remove the water and salts first, that is, put washing and drying right, and then set rust prevention and waiting times, because until the surface is clean and dry the effect of changing the preventive cannot be compared fairly.

Limits and cautions

Control concentrations for coolant and preventive, preventive grades and how long parts may wait unprotected differ with material, surface condition, plant climate and product, so numeric decisions follow each product's TDS and supplier guidance and are confirmed on real parts. For rust on functional faces such as bearing raceways or sealing faces, do not decide on the floor whether to wipe and use or to remachine; get the quality engineer's judgement. If rust has led to plating or heat-treatment defects, check the quality of that operation separately even after the rust is removed.

Safety matters too. For coolant, cleaners and preventives, follow the product's safety data sheet, the SDS, for gloves, eye protection and ventilation. Avoid prolonged skin contact with water-miscible coolants and preventives and avoid breathing their mist, and keep solvent-based preventives away from ignition sources with good ventilation. When grinding or wiping off rust, avoid breathing the dust.

Sources

  1. ASTM International. (2021). ASTM D1401-21, Standard test method for water separability of petroleum oils and synthetic fluids. https://webstore.ansi.org/standards/astm/astmd140121
  2. ASTM International. (2022). ASTM D4627-22, Standard test method for iron chip corrosion for water-miscible metalworking fluids. https://store.astm.org/d4627-22.html
  3. ASTM International. (2024). ASTM D1748-24, Standard test method for rust protection by metal preservatives in the humidity cabinet. https://store.astm.org/d1748-24.html
  4. Eppert, J., DeVor, R., Kapoor, S., & Rajagopalan, N. (2003). The effect of chip adsorption on selective depletion from a multicomponent synthetic metalworking fluid. University of Illinois at Urbana-Champaign, IDEALS. https://www.ideals.illinois.edu/items/110202
  5. Greenspan, L. (1977). Humidity fixed points of binary saturated aqueous solutions. Journal of Research of the National Bureau of Standards, 81A(1), 89–96. https://doi.org/10.6028/jres.081A.011
  6. Health and Safety Executive [HSE]. (2021). MW5, Managing fluid quality: COSHH essentials for machining with metalworking fluids. https://www.hse.gov.uk/pubns/guidance/mw5.pdf
  7. International Organization for Standardization [ISO]. (2012). ISO 9223:2012, Corrosion of metals and alloys — Corrosivity of atmospheres — Classification, determination and estimation. https://www.iso.org/standard/53499.html
  8. International Organization for Standardization [ISO]. (2017a). ISO 12944-3:2017, Paints and varnishes — Corrosion protection of steel structures by protective paint systems — Part 3: Design considerations.
  9. International Organization for Standardization [ISO]. (2017b). ISO 8502-4:2017, Preparation of steel substrates before application of paints and related products — Tests for the assessment of surface cleanliness — Part 4: Guidance on the estimation of the probability of condensation prior to paint application.
  10. McGuire, N. (2016, September). Fundamentals of rust preventives used for temporary corrosion protection. Tribology & Lubrication Technology, 28–34. https://www.stle.org/images/pdf/STLE_ORG/BOK/LS/Metalworking/Fundamentals%20of%20RUST%20PREVENTIVES%20used%20for%20temporary%20corrosion%20protection.pdf
  11. National Physical Laboratory [NPL]. (n.d.). Temporary corrosion protection. Guides to Good Practice in Corrosion Control No. 7. Retrieved November 2026. https://www.npl.co.uk/electrochemistry/corrosion-guides
  12. Passman, F. J., & Küenzi, P. (2020). Microbiology in water-miscible metalworking fluids. Tribology Transactions, 63(6), 1147–1171. https://doi.org/10.1080/10402004.2020.1764684
  13. Pourbaix, M. (1974). Atlas of electrochemical equilibria in aqueous solutions (2nd English ed.). National Association of Corrosion Engineers.
  14. Revie, R. W., & Uhlig, H. H. (2008). Corrosion and corrosion control: An introduction to corrosion science and engineering (4th ed.). Wiley. https://doi.org/10.1002/9780470277270
  15. Schindelholz, E. J., Kelly, R. G., & Risteen, B. E. (2014). Effect of relative humidity on corrosion of steel under acidified artificial seawater particles (SAND2014-19627C). Sandia National Laboratories. https://www.osti.gov/servlets/purl/1367735
  16. Stratmann, M., & Streckel, H. (1990). On the atmospheric corrosion of metals which are covered with thin electrolyte layers—II. Experimental results. Corrosion Science, 30(6–7), 697–714. https://doi.org/10.1016/0010-938X(90)90033-2
  17. Tang, Z. (2019). A review of corrosion inhibitors for rust preventative fluids. Current Opinion in Solid State & Materials Science, 23(4), 100759. https://doi.org/10.1016/j.cossms.2019.06.003
  18. Vernon, W. H. J. (1935). A laboratory study of the atmospheric corrosion of metals. Part II.—Iron: The primary oxide film. Part III.—The secondary product or rust. Transactions of the Faraday Society, 31, 1668–1700. https://doi.org/10.1039/TF9353101668

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.