Why do deep internal passages rust when the outside is protected?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Corrosion Prevention

Dipping longer or switching to a heavier preventive is the usual response to rust inside passages, but a film protects only where the liquid reaches the metal and stays there, so where it cannot get in or has drained away, more time or strength tends not to stop the rust returning. What actually lies behind it can be a viscosity unsuited to the passage, air trapped at blind ends, an application method that misses the inside, a film thinned as it drains, or wash water left inside, and sometimes two or more at once.

Background

Some parts carry deep passages inside them: hydraulic blocks, valve bodies, pump housings, the cooling channels of moulds. The outside gleams with rust-preventive oil, yet an endoscope at incoming inspection finds brown rust deep in the passages, at blind ends and around cross-drillings. The inside is hard to clean, so the part has to be washed or machined again, and if it is assembled as it is, flakes of rust travel round the system. Loose rust can block valves, filters and instruments (Darwin et al., 2010).

A preventive film protects metal only where the liquid reaches it and stays there. Rust grows where a thin film of water sits on the surface with oxygen and ions dissolved in it, so a spot with no film can start rusting as soon as moisture gets in (Revie & Uhlig, 2008). Yet how deep a liquid soaks into a narrow hole grows with time and varies widely with the size of the hole and the liquid's surface tension and viscosity (Washburn, 1921). What happens by itself on the outside happens inside a passage only when geometry, liquid and method all suit one another.

So rust inside passages usually falls into three kinds of place: where the liquid never got in, where it got in and then thinned as it drained away, and where water took the place before the preventive did. Where in the passage the rust started narrows down which of the three it is a good deal.

When this kind of rust turns up, the technical team sets up the five hypotheses below and eliminates them one at a time. The first check never changes: look into the rusted passages with an endoscope or by sectioning, note how far from the entry the rust is, which way the surface faces and whether it is a blind end, and compare washing and drying, the application method, and the preventive's type and temperature with its technical data sheet, the TDS.

Hypothesis 1: viscosity mismatch

This hypothesis moves forward when a heavy preventive oil chosen for outside faces is used unchanged on parts with long, slender passages. The same goes for a cold preventive tank in winter, and at the other extreme for a very thin oil that runs out of the passages and leaves almost no film. Take a winter morning when hydraulic manifolds are dipped in a preventive tank beside an unheated store. The outside is thickly covered, but a few weeks later the customer reports brown rust inside the slender cross-drillings.

The distance a liquid soaks into a narrow hole grows with the square root of time and slows as viscosity rises, so the longer and narrower the passage, the longer the liquid takes to reach the end (Washburn, 1921). The viscosity of petroleum liquids changes strongly with temperature, and a standard sets out equations and charts for working out that relationship (ASTM International, 2020). In a cold tank the same product becomes much thicker and may not reach deep into the passages within the set dipping time. A liquid that is too thin, on the other hand, gets in easily but drains off after withdrawal and leaves a thin film (Jeffreys, 1930).

Check first whether rust worsens with distance from the entry. If it does, put the same oil at the same temperature into a test piece drilled to the same diameter, or a clear tube, and measure how far it gets in the set time. Log the tank temperature and confirm it fits the TDS application temperature and viscosity range. If the oil is suspected of being too thin, watch how much runs out of the passage entries over time after withdrawal. When endoscoping rusted parts, note at what depth the boundary between oily and dry wall lies; that makes comparison with the result after a change easier.

If viscosity does not suit, choose the product or conditions again to match the depth of the passages. For deep passages, review a low-viscosity grade or a solvent-thinned grade that soaks in well, confirming on test pieces how thick a film it leaves. Warm the tank into the TDS application temperature range, and set dipping time from the time it took to reach the end in the trial, plus a margin.

Hypothesis 2: trapped air pocket

If rust on parts with blind ends, such as blind holes, tapped holes and drillings closed with plugs, always starts at those ends, suspect air. It happens especially when the orientation of parts on hooks or in baskets is not fixed, and when dipping time is short. Consider valve bodies laid any which way in a basket and lowered into the tank. Bubbles rise briefly from some holes and then stop, the bottoms of the blind holes come out bare metal, and later the rust starts there too.

For liquid to enter a blind hole, the air inside has to leave first. Surface tension makes it hard for liquid to enter a small hole closed at one end, so much so that ways of removing the gas inside are a subject of research in their own right. The same study notes that existing methods of filling by vacuum or steam need pressure vessels and extra pressurising and depressurising steps (Matsumoto et al., 2022). When the entry faces down or sideways, the lighter air has no way up and stays put, like air in an upturned cup. The preventive never touches the place the air occupies, so when humid air later gets into that space, bare metal is what gets wet.

Dip a real part in preventive in a clear container in the same orientation and watch which holes release bubbles and when they stop. Put a thin swab or an endoscope into the blind ends of withdrawn parts to see whether preventive is there, and check whether the rust started at the bottom of the blind end and spread towards the entry. Comparing with parts dipped in another orientation makes the share due to air clear.

If air is the cause, give it a way out. Fix the hanging orientation so blind holes open upwards, and tilt or shake parts while immersed to drive bubbles out. For deep, small blind holes, fill from the bottom with a fine nozzle, and if that still fails, review filling under vacuum together with the equipment it needs. Put the chosen orientation into the work instruction as a drawing, so every shift dips parts the same way.

Hypothesis 3: unsuitable method

Look at this hypothesis when dipping has been replaced by spraying to keep pace with the line, when only outside faces are sprayed and passages get no separate treatment, and when fogging or a volatile corrosion inhibitor is used but the openings are left open. It weighs more if the change of method and the rise in rust complaints line up in time. A case in point is a plant that replaced its dip tank with spray nozzles over the conveyor. Outside faces still give no trouble, but complaints about rust inside the passages rose from then on.

Preventives can be applied by dip tank, spray, roller, brush or wiping, and the choice of method depends on the size and shape of the part (McGuire, 2016). Spray droplets fly straight from the nozzle, so they reach faces the nozzle can see but have trouble reaching the inside of bent or intersecting passages. A US military standard for storing industrial plant equipment called for internal surfaces that are not otherwise lubricated to be covered with a preventive compound by spraying or fogging, and for pipe ends to be closed with plugs (DoD, 2001). A volatile corrosion inhibitor protects by spreading as vapour through a closed space and clinging to the metal, so if the openings are left open or the space is too large, it falls short of the concentration it needs (Gangopadhyay & Mahanwar, 2018).

Match the date of the method change with the date rust complaints rose in the records. Treat one test part by the current method, then section it and mark where film is present and where it is not; that shows exactly how far the method reaches. Another way is to push thin strips of oil-absorbing paper into the passages to different depths and see whether they come out marked. If fogging or a volatile inhibitor is used, check too that openings were closed right after treatment and that the plugs fit.

If the method does not reach the passages, treat outside and inside separately. Outside faces can stay on spray, but passages are filled and drained or injected through a nozzle, and fogging is used only on parts whose openings can be closed. A volatile inhibitor works only when it vaporises inside a closed space and clings to the metal faces (Bastidas et al., 2005), so plug every opening after it goes in and confirm with the supplier that the product suits that metal.

Hypothesis 4: drained, thin film

Look at this hypothesis in processes that fill and drain passages with preventive, or dip parts and leave them hanging to drain for a long time, and with thin oils, solvent-thinned products and warm tanks. It applies especially when rust gathers on upward-facing walls or the upper part of vertical passages. Think of a mould block with long vertical cooling channels that are filled with preventive oil, drained and stood upright. After storage the endoscope shows oily walls low in the channel, while the walls near the upper entry have a shine close to bare metal.

A film on a surface withdrawn from liquid runs down under gravity. A long-established result shows that a film draining down a vertical surface is thicker the higher the viscosity, and thinner as time passes and the nearer it is to the top (Jeffreys, 1930). Preventives are usually designed to go on as a single coat 2 to 20 µm thick, the diluent can make up 80% to 95% of the liquid, and a solvent evaporates and stays out of the dried film (McGuire, 2016). With a film already designed to be thin, a little more drainage at the top leaves protection short, while liquid pools and stays thick at low points of bent passages.

Check whether rust has gathered on upward-facing walls, near entries or in the upper part of vertical passages. Stand flat test pieces treated the same way upright and after a set time press oil-absorbing paper against them at different heights; the marks show the difference between top and bottom even without numbers. Check in the process records how long parts drain, how long they hang and which way they face.

If the film appears to have drained away, adjust drainage time and orientation. Cut hanging time to what is needed, and turn parts that are thin at the top for a second pass or treat them twice. Review a grade that dries to a firm or tacky film, or a slightly more viscous one, checking on test pieces that it still soaks right to the end of the passages.

Hypothesis 5: wash water left inside

Look at this hypothesis when parts go through aqueous or high-pressure water washing, or water-based leak or pressure testing, after machining and only their outside is dried before rust prevention. The more cross-drillings and blind ends a part has, and the shorter the gap between washing and rust prevention on the line, the more it applies. Suppose a hydraulic block finishes its leak test, gets a blast of compressed air on the outside and goes straight into the preventive dip and the box. When the customer opens the box, rusty streaks run down below the ports.

Water in narrow passages and blind ends dries far more slowly than the outside, and inside a closed space the remaining water evaporates and tends to keep the humidity high (Darwin et al., 2010). One report put forward the hypothesis that corrosion found on transfer lines came mainly from high humidity and in some cases from residual hydrotest water, and examined whether drying the lines could reduce it (Shukla et al., 2024). The thin water film in the last stage of drying is a state in which oxygen reaches the metal over a short distance and rust can grow faster than under immersion (Stratmann & Streckel, 1990). Where the preventive cannot push all the standing water aside, its film only sits on the water and never reaches the metal.

Tilt each port of a washed or tested part downwards and see whether water runs out. Weighing parts before and after drying, and again just before rust prevention, gives a rough idea of the water left inside. Rusty streaks running down from the ports, or rust pooled at the low points of passages, put this hypothesis in front.

If leftover water is the cause, add a step that dries right through before rust prevention. Blow compressed air into each port in a fixed order, then dry to the blind ends with warm air or vacuum drying before applying the preventive. Water-based preventives do not displace water well, so do not use one straight on wet passages (McGuire, 2016); for parts that are hard to dry fully, review a water-displacing preventive with the supplier. Set an acceptance check for dryness in advance, such as the weight comparison or tilting the ports.

Finding the cause

Rather than investigating the five hypotheses one by one, sectioning a few rusted parts or looking inside with an endoscope is the quickest starting point. Put the process records for washing, drying and rust prevention, their methods and times, and the tank temperature alongside, and most of the hypotheses narrow on the first day. Comparisons with test pieces come after that.

The position of the rust is the biggest clue. Rust that worsens with distance from the entry points to a viscosity unsuited to the passage, and rust that starts at the bottom of blind ends points to trapped air. Rust gathered round bends the spray cannot reach points to the application method, rust on upward-facing walls and the upper parts of vertical passages points to a film thinned by drainage, and rust at low points with streaks below the ports points to wash water left inside.

If position alone does not settle it, run control trials. Treat identical parts changing only the dipping orientation, only the drying time or only the tank temperature, and keep them in the same place. Change only one thing at a time, or there is no telling which one worked.

The final check is to section a real part from the corrected process and see that the film runs the full length of the passages. Once the section checks out, keep parts from the same process for as long as real storage and transport take, then look again with an endoscope. For the first few shipments, get the customer's incoming inspection results and confirm the inside of the passages with them.

Sometimes there is more than one cause. Passages that hold water often hold air at their blind ends as well, and a thin oil that reaches the end of a passage easily still drains thin from the top after withdrawal. In such cases drain and dry right through first, then set orientation, viscosity and method in turn, because in wet passages the effect of changing the preventive cannot be compared fairly.

Limits and cautions

The right passage diameters and depths, preventive viscosity and application temperature, and dipping and drying times differ by part and product, so numeric decisions follow the preventive's TDS and supplier guidance and are confirmed on sections of real parts. For parts with cleanliness requirements, such as hydraulic, fuel and cooling components, the preventive itself can become contamination in the next process or the customer's system, so first confirm from the customer specification what preventive may remain and how it is removed. For passages where rust has already dug in, do not decide on cleaning alone; agree remachining or scrapping with the quality engineer.

Safety matters too. Follow each preventive's safety data sheet, the SDS, for gloves, eye protection and ventilation. Fogging solvent-based preventives carries a high risk of flammable vapour and inhalation, so keep ventilation and ignition control in place, and handle volatile inhibitor powders so they do not become airborne. When blowing passages out with compressed air, wear eye protection against spray and chips and never point the nozzle at anyone.

Sources

  1. ASTM International. (2020). ASTM D341-20, Standard practice for viscosity-temperature equations and charts for liquid petroleum or hydrocarbon products. Reapproved 2025. https://store.astm.org/d0341-20r25.html
  2. Bastidas, D. M., Cano, E., & Mora, E. M. (2005). Volatile corrosion inhibitors: A review. Anti-Corrosion Methods and Materials, 52(2), 71–77. https://doi.org/10.1108/00035590510584771
  3. Darwin, A., Annadorai, K., & Heidersbach, K. (2010). Prevention of corrosion in carbon steel pipelines containing hydrotest water – An overview (Paper No. 10401). CORROSION 2010. NACE International. https://doi.org/10.5006/C2010-10401
  4. Gangopadhyay, S., & Mahanwar, P. A. (2018). Recent developments in the volatile corrosion inhibitor (VCI) coatings for metal: A review. Journal of Coatings Technology and Research, 15(4), 789–807. https://doi.org/10.1007/s11998-017-0015-6
  5. Jeffreys, H. (1930). The draining of a vertical plate. Proceedings of the Cambridge Philosophical Society, 26(2), 204–205. https://doi.org/10.1017/S0305004100015437
  6. Matsumoto, Y., Mizushima, Y., & Sanada, T. (2022). Removing gas from a closed-end small hole by irradiating acoustic waves with two frequencies. Micromachines, 13(1), 109. https://doi.org/10.3390/mi13010109
  7. McGuire, N. (2016, September). Fundamentals of rust preventives used for temporary corrosion protection. Tribology & Lubrication Technology, 28–34. https://www.stle.org/images/pdf/STLE_ORG/BOK/LS/Metalworking/Fundamentals%20of%20RUST%20PREVENTIVES%20used%20for%20temporary%20corrosion%20protection.pdf
  8. Revie, R. W., & Uhlig, H. H. (2008). Corrosion and corrosion control: An introduction to corrosion science and engineering (4th ed.). Wiley. https://doi.org/10.1002/9780470277270
  9. Shukla, P. K., Fuentes, R. E., Wiersma, B. J., Girardot, C., Page, J., & Campbell, S. (2024). Effect of drying on corrosion mitigation of Hanford transfer lines (SRNL-STI-2024-00026). AMPP Annual Conference + Expo 2024. https://www.osti.gov/biblio/2322414
  10. Stratmann, M., & Streckel, H. (1990). On the atmospheric corrosion of metals which are covered with thin electrolyte layers—II. Experimental results. Corrosion Science, 30(6–7), 697–714. https://doi.org/10.1016/0010-938X(90)90033-2
  11. U.S. Department of Defense [DoD]. (2001). MIL-STD-107J, Preparation and handling of industrial plant equipment (IPE) for shipment and storage. Cancelled without replacement 2010. https://everyspec.com/MIL-STD/MIL-STD-0100-0299/MIL-STD-107J_20749/
  12. Washburn, E. W. (1921). The dynamics of capillary flow. Physical Review, 17(3), 273–283. https://doi.org/10.1103/PhysRev.17.273

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.