BlogApplication notes
Why does start-up with rust preventive still on smoke and plug filters?
- Type
- Application notes
- Published
- 23 November 2026
- Prepared by
- Jonghwan Moon
- Product group
- Corrosion Prevention
Starting up with the preservative film left on, on the assumption that the operating oil will dissolve it, is the usual response, but ‘temporary’ in a temporary rust preventive means only that it can be removed later, not that it dissolves in the operating oil, so a film left on can turn to smoke on hot surfaces and end up in the filters. What actually lies behind it can be a thick waxy film burning on hot surfaces, a film that does not dissolve in the operating oil, flakes of film breaking away, leftover solvent or over-application, and sometimes two or more at once.
Background
A few tens of minutes after power first goes on to a newly installed machine, white smoke rises from the parts that heat up and an acrid smell spreads across the shop. By the next day the pressure drop across the circulating oil filter has climbed and the clogging indicator is showing. Commissioning stops, days go on changing filters and cleaning out the system, and while the filter sits on its bypass valve, unfiltered oil goes back to bearings and valves. Workers breathe the smoke, and it can set off fire detectors or catch fire.
Most preventives applied before dispatch are temporary rust preventives. The classification standard for them states that temporary refers not to how long they work but to the fact that they can be removed after a time, and it groups them by the nature of the film: thin oily films, solvent-applied waxy or dry films, asphalt-like bituminous films, greases. Each group comes off differently. A thin oily film may not need removing at all, whereas a bituminous film needs a suitable solvent plus mechanical effort (ISO, 1987).
So start-up trouble splits two ways: the film takes heat on a hot surface and turns into smoke and residue, or it gets into the operating oil, travels around undissolved and lodges in filters and narrow passages. Which way it went shows first in where the smoke came from and in what the filter caught.
In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: find out from the shipping documents and labels which preventive was applied where, look up in that product's technical data sheet, the TDS, whether it must come off before operation and whether it may mix with the operating oil, and compare that with what was actually done.
Hypothesis 1: thick film burning
Equipment that has crossed the sea in export packing for months, and spare parts held in long storage, sometimes arrive wearing a thick waxy film on the outside. The trouble comes when that film stays on places that get hot in service: moulds and heated platens, rolls, the area around heaters, brake and clutch faces, motor and pump bodies, exhaust-side parts. Imagine the day the heaters on a newly installed extruder are first switched on. As the barrel warms, smoke curls up from gaps in the heater bands and around the die, and within an hour brown, sticky marks have baked onto those spots.
The smoke is tiny droplets of what evaporates from the film, condensing as it cools in the air. Oily material evaporates lighter molecules first as temperature rises, and the test for evaporation loss of lubricating oils heats the oil to 250°C for an hour and looks at the weight lost (ASTM International, 2021). What does not evaporate oxidises on the hot metal in contact with air, and as oxidation goes on it forms insoluble sludge and a varnish-like film (Mortier et al., 2010). So when a thick film is left on a hot surface, smoke appears first and brown baked-on marks after.
Find out where the smoke rises first. While the machine warms up, measure the surface temperature where the smoke comes from with an infrared thermometer, and look at and feel the thickness and state of the film left there. If smoke comes only from hot outside surfaces such as heater surrounds, moulds and motor bodies and the oil system shows nothing wrong, this hypothesis leads. Scrape off a little of the film as a sample, and check the service temperature limit and the removal method in the product's TDS.
The rule is to strip the film from surfaces that get hot before start-up. Wipe it off with the solvent or cleaner the TDS names, and check hard-to-reach gaps separately before running. Bring temperatures up in steps with ample ventilation, and watch the spots that smoke during the first heat-up. From the next shipment on, set the scope of preservation so that surfaces that get hot receive a thin, removable product or none at all.
Hypothesis 2: insoluble film
The setting for this hypothesis is a gearbox, hydraulic tank, bearing housing or pipework coated inside with preventive and then filled with operating oil on the assumption that the film will dissolve and mix in. It stands out more when commissioning happens in winter or the system runs with cool oil. Two weeks or so into operation, the inspection cover of a reducer is opened: beige lumps have settled on the bottom and in the corners, and the outside of the filter element is coated in something like soft paste.
In the classification standard, waxy and dry films are the kind removed with a suitable solvent or cleaner (ISO, 1987). Even a wax that dissolves a little in the operating oil leaves a problem. Wax dissolved in petroleum mixtures separates out into several solid phases as temperature falls (Lira-Galeana et al., 1996). Wax taken up near the hot gears can therefore come out of solution again and build up in the cooler filter, cooler, tank bottom and return lines.
Taking an oil sample and letting it cool is the simplest check. Put oil drawn at operating temperature into a clear bottle, leave it at room temperature or cooler, and see whether it clouds or wax settles to the bottom. Treat new oil the same way for comparison. How readily the oil passes through a membrane can be put in numbers with the standard test that filters dry lubricating oil through membrane filters (ISO, 2025). If what the filter caught smears soft on the fingers and melts when warmed, it is wax rather than hard flakes.
If the TDS required removal before operation, there is no way round draining the oil, stripping the film, cleaning out the system and refilling with fresh oil. In future, agree with the supplier on a preservative oil stated to be compatible with the operating oil for inside surfaces. For engines there is even a separate specification for a preservative oil that serves as the lubricant for storage and break-in running; products allowed to stay in service and products that must come off are made differently from the start (DoD, 1998).
Hypothesis 3: flaking film
Look at this hypothesis when a film that dries hard, or a peelable film, was used on internal surfaces that oil reaches, when the film hardened and cracked while the machine stood idle, or when cold transport made it brittle. Film breaks away where oil flows fast and parts vibrate: circulating lubrication systems, hydraulic units, between gear teeth. Cut open the element of a hydraulic unit whose clogging indicator turned red a few hours into running, and thin flakes like paint chips are lodged between the pleats.
Undissolved flakes ride with the oil until they catch in the tightest spot. As flakes pile up on the face of a filter, the oil's path narrows and the pressure drop rises, and smaller fragments pass through the filter to valve clearances and bearings. Solid contamination in hydraulic fluid is expressed as a code from the number of particles per millilitre larger than 4 µm, 6 µm and 14 µm (ISO, 2021). The guide to cleaning and flushing turbine lubrication systems treats contamination control during building and installation, and flushing before operation, as part of commissioning, and advises against leaving this work to inexperienced people (ASTM International, 2023). Flakes from a preservative film are exactly that kind of build-time contamination.
Looking directly at what the filter caught is the first check. Open the element and examine the catch under a magnifier: thin, angular flakes mean dried film that broke away, while soft lumps that melt point to wax. Count particles in an oil sample against new oil, and look inside the tank and piping for places where the film has come off. Matching the colour and texture of the flakes with a sample of the applied preventive confirms where they came from.
If flakes are the cause, empty the system by flushing. Circulate flushing oil faster than in service through a temporary fine filter, changing elements and carrying on until particle counts reach the target. Open tanks and piping wherever they can be opened and strip any film left inside. Where the equipment maker has a procedure, that procedure comes first (ASTM International, 2023). In future, keep dry or peelable films off internal surfaces that oil will reach.
Hypothesis 4: leftover solvent
Solvent is left behind when a solvent-thinned preventive is sprayed inside an enclosed space such as a gearbox or housing and closed up at once, when it was applied on a cold day and the solvent evaporated slowly, or when it was applied just before dispatch and packed immediately. Parts washed in solvent and assembled before they were dry are the same case. Take a reducer sprayed inside with preventive and filled with oil a day later. As it warms up, a faint white vapour and a solvent smell come from the breather, and the oil in the sight glass looks thinner than new oil.
A solvent-based preventive becomes a film only once its solvent has evaporated. The military specification, too, defines such products as compounds cut back in solvent, applied cold, that leave a film after the solvent evaporates (DoD, 1993). In an enclosed space the vapour has no way out, so solvent stays in the film and at the bottom. Such solvents have low flash points. Stoddard solvent, used in preventives and cleaning, has a flash point of 102 to 110°F, roughly 39 to 43°C (NIOSH, n.d.). The US Occupational Safety and Health Administration classes liquids with a flash point at or below 93°C as flammable liquids (OSHA, n.d.). When such vapour fills a space warmed by operation, vapour comes out of the breather, and solvent mixed into the operating oil thins it and so thins the oil film.
Smell is the quickest clue. Sniff for solvent at the breather and inspection ports, and measure the viscosity of an oil sample against new oil. A noticeably lower viscosity, or a flash point below that of new oil, means solvent has most likely mixed in. Find the dates of application, closing and oil filling in the records and compare them with the drying time in the TDS, together with the air temperature when the product was applied.
Once leftover solvent is confirmed, stop the machine and remove anything that could ignite it. Drain the contaminated oil, open the space and ventilate it to drive off the solvent, then refill with fresh oil. From then on keep to the drying time in the TDS, and inside enclosed spaces use a solvent-free preservative oil, or ventilate thoroughly after spraying before closing up.
Hypothesis 5: over-application
Suspect over-application when equipment in long storage was given another coat every few months, when parts were brushed or dipped heavily, or when the product was sprayed by eye with no set amount. Preventive that runs can also pool in oil holes, grooves and the bottom of housings. A machine tool that stood idle for over half a year and was resprayed with the same product every three months shows, on start-up day, preventive sagged and set along every lower edge and the mouths of its oil holes blocked.
This hypothesis is about quantity. The thicker the film, the more material there is to take heat and turn to smoke, and the more there is to pass into the operating oil and be filtered out. A solvent-based preventive forms its film only once the solvent has gone, so a new coat laid over a lower one before its solvent has evaporated traps that solvent underneath (DoD, 1993). Preventive that runs and pools blocks oil holes and narrow passages directly, and as it softens and washes out in service it adds to the load on the filter.
Inspect film thickness and the places where product has pooled. Scrape a set area of film from the same location and weigh it, or read the thickness with a film gauge, and compare the result with the coverage recommended in the TDS. If there is a record of recoating, count the coats, and go through the places where runs collect: lower edges, the mouths of oil holes, the bottom of housings. If smoke and filter plugging are worse on machines that were recoated more often, this hypothesis gains weight.
From the next storage period on, fix the amount and the method. Before recoating, strip the old film or inspect it and touch up only where needed, and record coverage against the TDS recommendation. Plug oil holes and lubrication passages before applying, and clear pooled preventive before start-up.
Finding the cause
Clear the five hypotheses starting with the easiest to check. Which product went where and how much of it is in the documents and the TDS, and the spots that smoke and what the filter caught can be seen the same day. Viscosity, particle counts and filterability need samples sent away, so they come next.
The first fork is whether the trouble is smoke or filters. Smoke only from hot outside surfaces, with the oil system sound, points to a thick film burning on hot surfaces. Plugged filters with no smoke point to a film that did not dissolve in the oil or broke away as flakes. Vapour from the breather and thinned oil point first to leftover solvent.
Next is the form of what the filter caught. Soft lumps that smear on the fingers and melt when warmed are wax that never dissolved or dissolved and set again; thin, angular flakes are dried film that broke away. If an oil sample clouds or drops wax when cooled, lean towards the insoluble film. Whatever the form, if it is worse on machines recoated more often, over-application is adding to it.
If that still does not settle it, run control trials. Of two machines of the same model, strip and clean one as the TDS says and start the other the way it has been done, then compare smoke and filter pressure drop. Change only one thing at a time, or there is no telling which one worked. Afterwards, log filter change intervals and particle counts on the same basis and compare them, and the job is done only when those figures have come back to normal for new equipment.
The hypotheses can overlap. A film applied too heavily can burn on hot surfaces, resist dissolving in the oil, break into flakes and hold solvent as well. In such cases check for leftover solvent first and remove the fire risk, then strip the film, clean out the system and repeat the start-up, because while film remains, the effect of changing filters or lowering temperatures cannot be compared fairly.
Limits and cautions
How to remove a preventive, whether it may mix with the operating oil, its drying time and coverage differ by product, so follow the product's TDS and the equipment maker's commissioning procedure. For equipment with set cleanliness requirements, such as turbines, compressors and large hydraulic systems, leave flushing and cleanliness acceptance to a specialist contractor or the maker. If the smoke came from electrical parts or insulation, the cause may be something other than the preventive, so check with the equipment maker.
Safety matters too. For preventives and cleaning solvents, follow the safety data sheet, the SDS, for gloves, eye protection, respiratory protection and ventilation. If smoke appears, stop the machine, move people back and wait until it clears, with an extinguisher to hand. Do no hot work such as welding or grinding near spaces holding solvent vapour, and strip film or change filters only after the machine is fully stopped and locked out.
Sources
- ASTM International. (2021). ASTM D5800-21, Standard test method for evaporation loss of lubricating oils by the Noack method. https://store.astm.org/d5800-21.html
- ASTM International. (2023). ASTM D6439-23, Standard guide for cleaning, flushing, and purification of steam, gas, and hydroelectric turbine lubrication systems. https://store.astm.org/d6439-23.html
- International Organization for Standardization [ISO]. (1987). ISO 6743-8:1987, Lubricants, industrial oils and related products (class L) — Classification — Part 8: Family R (Temporary protection against corrosion). https://www.iso.org/standard/13217.html
- International Organization for Standardization [ISO]. (2021). ISO 4406:2021, Hydraulic fluid power — Fluids — Method for coding the level of contamination by solid particles.
- International Organization for Standardization [ISO]. (2025). ISO 13357-2:2025, Petroleum products — Determination of the filterability of lubricating oils — Part 2: Procedure for dry oils. https://www.iso.org/standard/86970.html
- Lira-Galeana, C., Firoozabadi, A., & Prausnitz, J. M. (1996). Thermodynamics of wax precipitation in petroleum mixtures. AIChE Journal, 42(1), 239–248.
- Mortier, R. M., Fox, M. F., & Orszulik, S. T. (Eds.). (2010). Chemistry and technology of lubricants (3rd ed.). Springer.
- National Institute for Occupational Safety and Health [NIOSH]. (n.d.). NIOSH pocket guide to chemical hazards: Stoddard solvent. Centers for Disease Control and Prevention. Retrieved November 2026. https://www.cdc.gov/niosh/npg/npgd0569.html
- Occupational Safety and Health Administration [OSHA]. (n.d.). 29 CFR 1910.106, Flammable liquids. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/laws-regs/regulations/standardnumber/1910/1910.106
- U.S. Department of Defense [DoD]. (1993). MIL-PRF-16173E, Corrosion preventive compound, solvent cutback, cold-application.
- U.S. Department of Defense [DoD]. (1998). MIL-PRF-21260E, Lubricating oil, internal combustion engine, preservative and break-in.