Adding more concentrate or a second coat is the usual response to a white, patchy film, but a strong mix and a thick film can make the marks worse. What actually lies behind them can be hard dilution water, cold and damp drying, too strong a mix or too thick a film, film beading on leftover oil, or a dirty or diluted bath, and sometimes two or more at once.

Background

Parts fresh from the washer are dipped in a water-based rust preventive and hung on a rack. The next day some have dried to a thin, clear, even film, while others look cloudy, as if dusted with white powder, or carry a white ring wherever a droplet dried. Customers who inspect appearance treat these marks as defects, so stained parts have to be washed and treated again, costing delivery time and labour. An uneven film can also protect unevenly in storage, from one spot to the next.

A water-based rust preventive is a set of protective ingredients dissolved in water or dispersed in it as fine droplets, and what remains once the water leaves becomes the film. Water is cheap, carries no volatile organic compounds and evaporates completely without becoming part of the film, but drying is slow and impurities such as hard water minerals can cause trouble. It also does not displace water from the metal well, so extra cleaning may be needed to remove coolant residue left by earlier steps (McGuire, 2016).

For the film to come out clear and even, what remains must pack together without gaps as the water leaves. Ingredients dispersed as droplets or particles crowd together as the water evaporates, deform to fill the gaps and finally merge into one continuous film. When the process stops short and voids, grains or water stay inside the film, light scatters at their boundaries and the film looks white (Keddie & Routh, 2010). A white mark is therefore a signal of what got mixed into the film, or of where film formation stalled.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: keep a stained part and an evenly dried part side by side, log the date and time of treatment, the bath concentration, the source of the dilution water and the temperature and humidity where the parts dried, and compare them with the rust preventive's technical data sheet, the TDS.

Hypothesis 1: hard dilution water

If marks began after the dilution water changed, look at the water first. This is especially likely when mains water was swapped for well or process water, when softener regeneration has fallen behind, or in a bath that has been topped up with water alone as water evaporated from it. Picture the first week on a newly moved line, with the rust preventive mixed in process water. Flat faces look fine, but white rims form around holes where liquid pooled and dried and along the lower edge of each part, and a fingernail scrapes up powder.

Hard water is water with a lot of dissolved calcium and magnesium. When soap reacts with the calcium in hard water it forms a residue that does not dissolve readily, and the cloudy spots left on dishes also come from hard water (USGS, n.d.). In a rust preventive built on anionic ingredients such as fatty acid soaps, the same reaction can form calcium residue that ends up as white grains in the film, and dissolved minerals cannot leave with the evaporating water, so they stay where they were. Impurities such as hard water minerals are named as a source of trouble in water-based rust preventives too (McGuire, 2016). The white rim forms because the edge of a drying droplet stays pinned in place while liquid from the centre flows outwards to replace what evaporates at the edge, carrying dissolved and suspended matter to the rim (Deegan et al., 1997).

Water settles the question as soon as it is measured. The hardness of the dilution water can be measured with the standard test method that titrates it against a standard EDTA solution (ASTM International, 2025), and metalworking fluid guidance likewise advises checking incoming water for hardness, pH and bacteria and agreeing suitable water quality with the supplier (HSE, 2021). One classification calls water with up to 60 mg per litre as calcium carbonate soft, 121 to 180 mg hard and over 180 mg very hard (USGS, n.d.). Mix the same concentrate with site water and with deionised water, treat identical test pieces in each and dry them side by side; if only the deionised set comes out clean, the water is the cause.

If the water is the cause, the first step is to change it. Ask the supplier for the recommended water quality, and mix with softened or deionised water if needed. Topping up only with water as it evaporates keeps piling minerals into the bath, so top up with the specified water too. For parts that already carry white rims, check with the TDS or the supplier whether rinsing in clean water and treating again is the right route.

Hypothesis 2: cold, damp drying

When the bath and the water are the same but marks come and go with the season or the weather, suspect the drying conditions. The poorly heated warehouse end in winter, the rainy season, spots near an outside door and corners with no air movement all qualify, as does treating cold stock straight after it comes in. Say parts treated on a rainy-season evening were left stacked in their baskets overnight. Next morning the top parts are dry, but those deep in the basket and the faces where parts touch are still tacky or cloudy.

Evaporation depends on how much more moisture the surrounding air can take up, so it slows as air gets colder and damper (Keddie & Routh, 2010). Water-based rust preventives are slow to dry to begin with (McGuire, 2016), and the longer drying takes, the longer water sits on the metal. A part colder than the air makes things worse. If the surface is near the dew point, the temperature at which moisture in the air starts to condense, fresh water forms instead of drying off, which is why steel is expected to be at least 3 °C above the dew point before painting unless otherwise agreed (ISO, 2017).

Film formation depends on temperature too. Below a certain temperature, ingredients in particle form, such as emulsions, cannot fuse together even after the water has gone; that threshold is the minimum film formation temperature, or MFFT, and it is measured by a standard method (ASTM International, 2023). A film dried below it keeps voids between particles and turns white and powdery, or cracks (Keddie & Routh, 2010). Even a fully dried film can cloud over again if it holds water for long. One study of acrylic emulsion films linked this whitening to emulsifier left inside the film drawing water in (Luo & Huang, 2020).

Put a thermohygrometer where parts dry and match its log against the times stained parts were treated. Measure the part surface temperature with a contact thermometer and compare it with the dew point at the time, and check the minimum application temperature and drying time in the TDS. Dry half of one batch in the usual place and half somewhere warm with moving air, and the difference shows at once. Marks only where parts overlap mean air never reached those faces.

If the log shows the marks lining up with cold, damp hours, give the water a quick way out. Blow air across the drying area, warm air if needed, and let cold stock reach room temperature before treating it. Do not stack or pack parts until they are fully dry, and allow longer drying times in winter and the rainy season. If the product must work at low temperature, choose a grade suited to it with the supplier.

Hypothesis 3: too strong or too thick

Thick white bands where liquid collects, at the lower edge, at corners and round holes, point towards concentration and film thickness. Typical cases are adding concentrate after seeing marks, topping up an evaporating bath with concentrate alone, standing parts upright straight out of the bath with no time to drain, and spraying twice over the same area. Think of a bath left uncovered over the weekend and used as it is on Monday. Upper faces dry thin and clear, but where liquid ran down and collected the film is thick and white, with a fine net of cracks.

A water-mixed fluid grows stronger in use as water evaporates, which is why metalworking fluid guidance advises topping up with a mix weaker than the recommended concentration (HSE, 2021). A strong mix leaves more solids once dry, so the film grows thicker, and ingredients that can no longer stay dissolved as the water leaves may be left behind as crystals, a white powder. Thickness is a problem in itself. As a dispersion dries, capillary pressure builds in the layer that is setting (Routh, 2013), and experiment and theory have shown that above a certain thickness the film cannot bear this stress and cracks (Singh & Tirumkudulu, 2007). Cracks and crystals scatter light and look white, and moisture can reach the metal through the cracks.

Measure bath concentration with a refractometer and compare it with the TDS range. Metalworking fluid guidance calls for weekly checks of concentration and pH and for keeping to the supplier's recommended levels (HSE, 2021). Compare the amount of film by weighing identical test pieces before and after treatment, and see whether the white band sits only at the lower edge or covers the whole face. Only at the lower edge points to draining and pooling first; an evenly white face points to concentration.

If the concentration is high, bring it back within the TDS range, and correct a bath that strengthens through evaporation with water or a weak mix. Hang parts at an angle so they drain and give them a moment, or blow pooled liquid off with compressed air. If a heavier film is needed, agree a method the TDS allows with the supplier rather than applying one strong coat. Wash off a film that has already cracked and treat again.

Hypothesis 4: film beading on oil

Marks that form as droplet-shaped islands or streaks, with bare metal showing between them, suggest oil left on the surface. Look at this hypothesis when the cleaner is spent or running cold, when oil floats on the wash tank, for parts that carried hard-to-remove oils such as press oil or an earlier rust preventive, and for parts handled bare-handed after washing. A typical scene comes in a week when the washer filter is overdue: liquid on a part lifted from the rust preventive does not cover it smoothly but quickly pulls back into small beads. Once dry, a white ring marks the spot where each bead sat.

Water spreads widely on clean metal, but it wets an oil-covered surface poorly, so a spread water film pulls itself back and breaks into drops. This break-up of a liquid film is called dewetting (de Gennes, 1985). In rust preventives the diluent can make up 80% to 95% of the finished fluid, and in water-based products that diluent is water (McGuire, 2016), so on oil the rust preventive film breaks up in the same way. As the drops dry, solids gather at their edges into rings (Deegan et al., 1997), while the bare metal between drops is left with almost no film, so marks and rust can appear together.

The water-break test, pouring clean water over a washed part, is an easy check. A water film that covers evenly without breaking means a clean surface; water that splits and leaves dry patches means a water-repelling contaminant is still there. The standard notes that the method can reveal oil only molecules thick, but that its sensitivity drops markedly on very rough or porous surfaces and that it is a go or no-go test rather than a measurement (ASTM International, 2021). Log the cleaner concentration, temperature and floating oil alongside the result.

If oil turns out to be the cause, fix the cleaning rather than the rust preventive. Bring cleaner concentration and temperature back within the cleaner's TDS range, skim oil off the wash tank and rinse more. Do not handle washed parts bare-handed, and add the water-break test to routine checks. Treat a clean surface as the starting point rather than expecting the rust preventive to clean.

Hypothesis 5: dirty or diluted bath

Marks that increase the longer a bath is used and ease off for a while after it is changed point to the bath itself. Baths that take wet parts straight in, so that cleaner and rinse water keep coming in with them, baths with floating oil or sludge on the bottom, uncovered baths collecting dust and baths that have started to smell all qualify. Stand in front of a bath nearing its change date. A rainbow sheen of oil drifts on the surface, parts come out with that oil on them, and the dried film is patchy and tacky in places.

In dip application, water carried in on parts can mix with the rust preventive and reduce its protection (McGuire, 2016). The bath thins as water comes in, and a thinner liquid leaves less solids in the same dipping time, so the film comes out thin and uneven. For water-mixed metalworking fluids, the UK Health and Safety Executive notes that the fluid stays in the machine and deteriorates over time and can be contaminated with tramp oil, fines and bacteria (HSE, 2021). A water-based rust preventive bath calls for the same care, and floating oil picked up by parts on the way out leaves the same beaded marks as leftover oil from washing.

This time read the refractometer for a value below the TDS range, and check pH, surface oil, sludge and smell at the same time. Bacteria can be checked with dipslides, a culture test strip, and metalworking fluid guidance reads a dipslide result of 10,000 cfu per ml or more as a sign of microbial growth (HSE, 2021). Dip identical test pieces in freshly made liquid and in the working bath and dry them side by side, and it is clear at once whether the bath is to blame.

If only the fresh liquid dries clean, start by cutting the water that parts bring in. Shake or blow off water after washing and rinsing before dipping, skim floating oil, filter out sludge and cover the bath when it is idle. Measure and log concentration and pH at set intervals, and when they drift out of range or smell and sludge build up, change the bath and clean the tank as the TDS and the supplier direct.

Finding the cause

Five hypotheses do not mean five separate investigations. Rule them out one at a time, starting with what records and simple measurements can show. Bath concentration, dilution water hardness and the temperature and humidity where parts dry can be measured the same day, and a water-break test takes minutes. Bath contamination comes next, together with control trials using test pieces.

The shape and position of the marks are the first clue. A white ring wherever a droplet dried, starting after a change of dilution water, points to hard water; thick bands with fine cracks at lower edges and corners point to a strong mix or a thick film; and bare metal between bead-shaped islands points to leftover oil. Cloudiness only on overlapping faces and deep in baskets points to slow drying, and marks that grow as a bath nears its change date and fall back once it is changed point to the bath.

When the marks appear is a clue as well. Marks that come and go with season and weather point to drying conditions; marks only on certain materials or after a certain earlier step point to cleaning. Marks that creep up day by day point to concentration rising through evaporation or to bath contamination. Comparing the first and last parts dipped in a single batch shows whether the bath changes during a run.

If that still does not settle it, run control trials that change one thing at a time. Mix the same concentrate with deionised water and with site water, compare fresh liquid with the working bath, dry somewhere warm and airy against the usual place, and treat parts given an extra wash alongside normal ones. Change only one thing at a time, or there is no telling which one worked. The final check is whether parts treated under the corrected conditions dry evenly over several days and batches, and whether they pass the rust test agreed with the supplier.

The hypotheses can overlap. A bath mixed with hard water concentrates its minerals as it evaporates, and on cold, damp days thick spots and oily spots stay wet longer, so the marks spread. In such cases put the base right first, the cleaning and the dilution water the film sits on, and then set concentration and drying conditions, because while the base is unsettled the effect of changing concentration or drying cannot be compared fairly.

Limits and cautions

Suitable concentration, dilution water quality, drying temperature and time, and film thickness differ by product and part, so numeric decisions follow the rust preventive's TDS and the supplier's guidance. Whether a white mark is only cosmetic or has also cut protection cannot be judged by eye, so for parts with delivery requirements confirm it with the agreed rust test and the customer's criteria. For parts where rust has already started, set a separate procedure for dealing with the rust before reapplying the preventive.

Handle rust preventive concentrate and cleaners with gloves and eye protection as the product's safety data sheet, the SDS, directs. Water-mixed metalworking fluids are known to cause dermatitis on skin contact and lung diseases such as occupational asthma when mist is breathed in (HSE, 2021), so provide extraction and limit skin contact when spraying a water-based rust preventive as well. Dispose of spent liquid and tank sludge under local rules.

Sources

  1. ASTM International. (2021). ASTM F22-21, Standard test method for hydrophobic surface films by the water-break test. https://store.astm.org/f0022-21.html
  2. ASTM International. (2023). ASTM D2354-10(2023), Standard test method for minimum film formation temperature (MFFT) of emulsion vehicles. https://store.astm.org/d2354-10r23.html
  3. ASTM International. (2025). ASTM D1126-17(2025), Standard test method for hardness in water. https://store.astm.org/d1126-17r25.html
  4. de Gennes, P. G. (1985). Wetting: Statics and dynamics. Reviews of Modern Physics, 57(3), 827–863. https://doi.org/10.1103/RevModPhys.57.827
  5. Deegan, R. D., Bakajin, O., Dupont, T. F., Huber, G., Nagel, S. R., & Witten, T. A. (1997). Capillary flow as the cause of ring stains from dried liquid drops. Nature, 389(6653), 827–829. https://doi.org/10.1038/39827
  6. Health and Safety Executive [HSE]. (2021). MW5: Managing fluid quality. COSHH essentials for machining with metalworking fluids. HSE. https://www.hse.gov.uk/pubns/guidance/mw5.pdf
  7. International Organization for Standardization [ISO]. (2017). ISO 8502-4:2017, Preparation of steel substrates before application of paints and related products — Tests for the assessment of surface cleanliness — Part 4: Guidance on the estimation of the probability of condensation prior to paint application. ISO.
  8. Keddie, J. L., & Routh, A. F. (2010). Fundamentals of latex film formation: Processes and properties. Springer. https://doi.org/10.1007/978-90-481-2845-7
  9. Luo, Z., & Huang, H. (2020). Glass-transition temperature of a polyacrylate latex film and its water whitening resistance. Journal of Applied Polymer Science, 137(6), 48361. https://doi.org/10.1002/app.48361
  10. McGuire, N. (2016, September). Fundamentals of rust preventives used for temporary corrosion protection. Tribology & Lubrication Technology, 28–34. https://www.stle.org/images/pdf/STLE_ORG/BOK/LS/Metalworking/Fundamentals%20of%20RUST%20PREVENTIVES%20used%20for%20temporary%20corrosion%20protection.pdf
  11. Routh, A. F. (2013). Drying of thin colloidal films. Reports on Progress in Physics, 76(4), 046603. https://doi.org/10.1088/0034-4885/76/4/046603
  12. Singh, K. B., & Tirumkudulu, M. S. (2007). Cracking in drying colloidal films. Physical Review Letters, 98(21), 218302. https://doi.org/10.1103/PhysRevLett.98.218302
  13. U.S. Geological Survey [USGS]. (n.d.). Hardness of water. Water Science School. Retrieved November 2026. https://www.usgs.gov/water-science-school/science/hardness-water

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.