Jonghwan Moon
Product group
Corrosion Prevention

Recoating more heavily is the usual response to a cracked, flaking wax film, but a thick film can crack and lift more readily. What actually lies behind it can be cold embrittlement, too thick a film, handling before the film is dry, oil or water on the surface beneath, or vibration and bending in transit and assembly, and sometimes two or more at once.

Background

Shafts, moulds or flanges sent out with a rust-preventive wax turn up again in a warehouse or at a customer's site. A net of fine cracks has spread across what was a smooth film, and at edges and contact points the film has lifted like scales and fallen away. Where the film is gone, bare metal meets air and moisture directly, so rust can start there in storage, and rusted parts must be cleaned and recoated or taken back. Flakes of wax also end up on packaging and other parts and have to be cleaned off.

A rust-preventive wax is a temporary protective in which wax and inhibitors such as metal sulfonates are dissolved in a solvent or oil. In solvent types, what remains once the solvent evaporates becomes the film; such preventives are typically applied as a single coat 2 to 20 µm thick and removed once they have served their purpose. Wax is highly crystalline with a flaky texture, and oxidised wax has lower crystallinity and a smoother texture (McGuire, 2016). A film cracks when the stress built up in it exceeds what the film can bear, and flakes off when that stress, or a force from outside, exceeds the bond between film and metal.

Stress reaches the film by several routes. As the solvent leaves, the film tries to shrink, but a film stuck to metal cannot shrink freely, so tensile stress builds up inside it (Francis et al., 2002); a change in temperature makes film and metal expand and contract by different amounts, adding stress; and when a part bends or vibrates, the film has to stretch with it (Croll, 2022). Cracking and flaking therefore narrow down quickly once it is clear whether the film has weakened, the stress has grown, or the bond has weakened.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: keep a cracked part and a sound one together, log the date and method of application, the temperatures where the wax was applied and where the parts were stored, and the shipping route, and compare them with the wax's technical data sheet, the TDS.

Hypothesis 1: cold embrittlement

If cracking clusters in winter, or appears only on parts that went through an unheated warehouse, an outdoor yard or winter sea freight, look at temperature first. Parts coated in a warm shop and moved straight into the cold, and parts lifted or knocked while the film was stiff, belong to the same group. Take a day when wax-coated flanges stacked in an outdoor store in midwinter are moved by forklift. Where the forks touch an edge, the film cracks like glass and drops away in pieces, while the same parts brought indoors a few days earlier only show a dent when pressed.

Wax is vulnerable to cold because of its crystal structure. A study that measured the tensile properties of paraffin wax between 10 and 30 °C found higher modulus and maximum stress at lower temperatures, with behaviour changing as the wax passed into softer crystalline states on warming. The same study traced wax's ductility at room temperature to its closeness to these intermediate states, and attributed the much greater ductility of wax blended with clay to a lower brittle-ductile transition temperature, the point below which the material breaks instead of stretching (Wang et al., 2007). Put the other way round, a wax film cooled below that transition grows stiffer but can barely stretch, so it breaks. On top of this, film and steel contract by different amounts as temperature falls, adding stress, and even small stresses like these can start failure when they repeat or concentrate in one spot (Croll, 2022).

Check the lowest temperatures along the storage and shipping route from the records and compare them with the application and storage temperature ranges in the TDS. See whether the cracks gather where parts were knocked or lifted, and whether they remain after the parts warm up. Coat thin steel test panels with the same wax, keep one set at room temperature and one at the storage temperature, then bend them round a cylindrical mandrel; it is immediately clear whether only the cold set cracks. The bend test is the standard method for judging how well an attached coating resists cracking as it is stretched (ASTM International, 2021a).

If cold proves to be the cause, cut the time the film spends cold, or use a wax that holds up when cold. Move winter storage out of wind and frost, and use padding to soften knocks when cold parts are lifted or moved. If cold transport cannot be avoided, give the supplier the lowest transport temperature and choose together a grade whose flexibility is assured at that temperature.

Hypothesis 2: film too thick

Cracks that divide the film into polygons like drying mud, gathered where wax collects, at lower edges, in grooves and at corners, are a sign of thickness. Heavy films come from using wax that has cooled or lost solvent and thickened, from long dips or standing parts upright with no time to drain, and from pouring or spraying one heavy coat instead of two thin ones. On a cold morning, for instance, parts dipped in a wax bath that thickened as it cooled overnight come out with a heavier coat than usual, and a few days later cracking starts at the thick lower edges.

Thickness is a risk in itself. Thin-film fracture mechanics shows that, at the same stress, the energy available to drive a crack or a debond in a film attached to metal rises as the film gets thicker, so a thick film can crack and peel at a stress a thin film survives (Hutchinson & Suo, 1991). Nor is the stress inside a thick film any lower. Films shrink both while they set and after, tensile stress builds up as far as the metal restrains that shrinkage, and molecular motion relieves only part of it (Francis et al., 2002). Rust preventives are designed to go on as a single coat typically 2 to 20 µm thick (McGuire, 2016), so spots where wax has pooled far thicker are outside the use they were designed for.

Compare film thickness where it cracked and where it is sound. Film on steel can be measured with a magnetic thickness gauge, and without one, weigh identical test pieces before and after coating to compare the amount of film. Check the bath temperature, viscosity and solvent top-up records against the TDS ranges, and look for runs and pooled spots after coating. Cracks only in thick areas, with thin areas sound, make thickness the likely cause.

If thickness is the problem, first bring the liquid back to the temperature and viscosity set in the TDS. Replace evaporated solvent by the specified method, hang parts at an angle so pooled wax runs off, and blow out liquid left in grooves and holes. If longer protection calls for a heavier film, agree with the supplier on a grade made for thick films or on building it up in thin coats rather than applying one heavy coat.

Hypothesis 3: handled before dry

If the film has torn along handprints, strap marks or packaging patterns, or cracks start from pressed spots, suspect handling before the film was dry. It happens when parts are stacked and wrapped straight after coating to make a shipment, on cold or still days when solvent leaves slowly, and when a thick film takes long to dry through. Consider parts coated late in the afternoon for an evening shipment, stacked on a pallet and stretch-wrapped while only the surface was dry. When the wrap comes off at the destination, the film on contact faces tears away with it, and fine cracks ring the pressed spots.

In a solvent-type wax, drying means the solvent leaving the film. The solvent evaporates and is not part of the dried film (McGuire, 2016), but it leaves from the surface, so the surface can dry first while the inside stays soft for some time. The standard method likewise treats drying as a series of stages, from a surface that no longer marks to the touch to a film hard all the way through, and gives procedures for judging drying in the shop and field as well as at controlled laboratory temperature and humidity (ASTM International, 2022). A film still soft inside deforms and tears easily under pressure, and since films keep shrinking while they set and after, building up stress (Francis et al., 2002), spots pressed or scuffed before drying can remain weak points where cracks start once the film is fully dry.

The first thing to check is time. Compare the stage-by-stage drying times in the TDS with the actual time from coating to stacking and packing, and note the temperature and air movement where the wax was applied that day. Press the film with a finger at set intervals after coating and record when it stops taking a mark, which gives the drying time under shop conditions. Check whether torn and cracked spots coincide with where packaging, straps and supports touched.

If parts have been stacked and packed sooner than the drying time measured on the floor, build dedicated drying time into the process. Provide racks so coated parts hang without touching, move air across them so the solvent can leave, and extend drying time on cold days and for thick films. Hold stacking and packing until the drying time measured on the floor has passed, and for urgent shipments review a faster-drying grade with the supplier.

Hypothesis 4: oil or water beneath

A film that lifts in whole sheets without cracking, or slides off like a skin when pushed with a hand, over an oily or wet surface, points to what lies beneath it. Typical cases are skipping the wash and coating straight over cutting or press oil, water left in grooves and holes after washing, and coating cold parts in a warm, humid area. One example is wax sprayed on parts fresh from the washer with water still beaded in the grooves. A few days later the film round those grooves alone has blistered and lifted, and underneath the metal is damp or already rusting.

How well a film holds depends on what lies between film and metal. The classic explanation of poor adhesion holds that when a weak boundary layer such as oil or water sits at the interface, the bond fails in that layer (Bikerman, 1967). However hard the wax film, it cannot hold more firmly than the oil or water layer beneath it. Ingredients such as sulfonates are added to cling to the metal and drive water off, and many solvent-type preventives are made to go on over oily or damp surfaces (McGuire, 2016), but they cannot be expected to clear water pooled in a groove or a thick layer of oil. If the part surface is near the dew point, fresh water can condense even during coating, which is why steel is expected to be at least 3 °C above the dew point before painting unless otherwise agreed (ISO, 2017).

Peel back a little of the lifted film and wipe beneath it with a finger or filter paper, and it shows at once whether the culprit is oil or water. On washed parts, run the water-break test, pouring clean water over the part to see whether the film stays even and unbroken. The test can reveal very thin oil films but is a go or no-go check whose sensitivity drops on rough or porous surfaces (ASTM International, 2021b). Where coating takes place, measure and log the part surface temperature and the dew point of the air together.

If the wipe beneath the film comes up oily or wet, rebuild the preparation before coating. The solvent cleaning standard for coating work requires visible oil, grease, soil, drawing compounds, cutting compounds and similar contaminants to be removed with solvent, vapour, cleaning compound, alkali, emulsifying agent or steam, whichever suits (SSPC, 2015). After washing, blow water out of grooves and holes with compressed air and dry fully before coating, and coat cold parts only once they are well above the dew point. Strip film that has already lifted and treat the surface again from the start.

Hypothesis 5: vibration and bending

If the cracks run parallel in one direction, or gather where supports and straps touched or where the part flexes, suspect mechanical forces in transit and assembly. Parts that flex easily such as thin sheet and long bar, parts on long road or sea journeys, and parts bent or clamped during assembly after waxing are the usual candidates. Imagine thin steel brackets, waxed and then hauled a long way over rough roads. Rows of fine cracks have formed where they rocked on bearers and along the flexed edges, and the pieces of film between cracks are lifting from their edges and falling away.

A film attached to metal has to stretch when its substrate bends. The standard bend test notes that a coating is stretched when its substrate changes dimension, is bent during manufacture or is abused in service, and rates as flexibility the coating's ability to stretch without cracking (ASTM International, 2021a). Vibration in transit repeats this stretching countless times, and small stresses from bending or differing thermal contraction can start failure when they repeat or concentrate in one spot (Croll, 2022). Once a crack forms, debonding can spread from its tip along the interface between film and metal (Hutchinson & Suo, 1991), so the film between cracks drops off in pieces. A film stiffened by cold has even less room to stretch, so it cracks more readily under the same shaking.

Match the direction and position of the cracks against photos of the transport packing, the support positions and the assembly process. The clues are whether cracks run parallel to the bending axis, cluster where supports and straps touched, or start where parts were bent or clamped in assembly. Running coated test panels through the mandrel bend test and noting the diameter at which the film cracks lets you compare in figures how much bending a film can take (ASTM International, 2021a). Comparing the same parts stored without being shipped also helps.

If vibration and bending are the cause, the first step is to keep parts from moving. Secure parts firmly in their transport packing, pad the points where supports and straps touch, and shorten the span between supports so long parts do not sag. Where parts are bent or clamped in assembly, apply the wax after assembly where possible. If bending cannot be avoided, choose a more flexible grade with the supplier based on bend test results.

Finding the cause

Rather than investigate the five hypotheses one by one, strike out first what the records can rule out. The time between coating and shipment, the lowest temperatures in storage and transit, and the temperature and viscosity of the wax bath are usually already logged or can be measured at once. Film thickness and the water-break test come next, and transport conditions come last, since they mean checking the packing and the route.

The pattern of the damage is the first clue. Polygonal, mud-like cracking only where wax pooled points to a thick film, and parallel cracks gathered at supports or flexing zones point to vibration and bending. A film lifting in whole sheets without cracks, over an oily or wet surface, points to the surface beneath, and tears that follow handprints or packaging patterns point to handling before drying. Sharp, glass-like flakes found only on parts that passed through the cold point to cold embrittlement.

Timing helps sort them too. Damage already present when the packing is opened just after shipment points to drying or packing; damage that rises only in winter points to temperature; and damage only on parts that travelled far points to vibration. A film sound soon after coating that cracks gradually over time points first to stress building up from thickness, or to a weak bond on the surface beneath.

If that still does not settle it, run control trials on test panels. Coat the same wax at the specified thickness and at a heavy thickness, on cleaned and oily surfaces, and fully dried against under-dried, then bend them on a mandrel at room temperature and at the storage temperature. Change only one thing at a time to find which condition makes the cracks. The final check is to send real parts coated under the corrected conditions along the same route and see that the film arrives intact.

The hypotheses can overlap. A thick film dries slowly and so is more likely to be handled before it is dry, a film stiffened by cold cracks more readily under the same vibration, and a film over leftover oil lifts widely from even a small crack. In such cases put right first what is fixed at the coating step, the surface beneath and the thickness, and then look at drying, storage temperature and transport in turn, because while the coating step is unsettled the effect of changing storage or transport cannot be judged fairly.

Limits and cautions

Suitable film thickness, drying time, and application and storage temperatures differ by wax grade and application method, so numeric decisions follow the product's TDS and the supplier's guidance. Whether film damage shortens protection cannot be judged by eye alone, so for long-term storage or export parts confirm it with a rust test agreed with the supplier. Wax is a temporary protective that has to be removed before the next process, so when changing grade, also check how it comes off and how it affects the next step.

Many solvent-type rust-preventive waxes give off flammable vapour, so follow the product's safety data sheet, the SDS, on ventilation and ignition control, and provide extraction and respiratory protection when spraying. Wear gloves and eye protection to keep the product off skin and eyes, and collect solvent and rags used to strip or recoat wax in designated containers for disposal under local rules. When changing how heavy or long parts are packed and shipped, follow the site's safety rules on securing and lifting loads.

Sources

  1. ASTM International. (2021a). ASTM D522/D522M-17(2021), Standard test methods for mandrel bend test of attached organic coatings. https://store.astm.org/d0522_d0522m-17r21.html
  2. ASTM International. (2021b). ASTM F22-21, Standard test method for hydrophobic surface films by the water-break test. https://store.astm.org/f0022-21.html
  3. ASTM International. (2022). ASTM D1640/D1640M-14(2022), Standard test methods for drying, curing, or film formation of organic coatings. https://store.astm.org/d1640_d1640m-14r22.html
  4. Bikerman, J. J. (1967). Causes of poor adhesion: Weak boundary layers. Industrial & Engineering Chemistry, 59(9), 40–44. https://doi.org/10.1021/ie51403a010
  5. Croll, S. G. (2022). Stress and embrittlement in organic coatings during general weathering exposure: A review. Progress in Organic Coatings, 172, 107085. https://doi.org/10.1016/j.porgcoat.2022.107085
  6. Francis, L. F., McCormick, A. V., Vaessen, D. M., & Payne, J. A. (2002). Development and measurement of stress in polymer coatings. Journal of Materials Science, 37(22), 4717–4731. https://doi.org/10.1023/A:1020886802632
  7. Hutchinson, J. W., & Suo, Z. (1991). Mixed mode cracking in layered materials. Advances in Applied Mechanics, 29, 63–191. https://doi.org/10.1016/S0065-2156(08)70164-9
  8. International Organization for Standardization [ISO]. (2017). ISO 8502-4:2017, Preparation of steel substrates before application of paints and related products — Tests for the assessment of surface cleanliness — Part 4: Guidance on the estimation of the probability of condensation prior to paint application. ISO.
  9. McGuire, N. (2016, September). Fundamentals of rust preventives used for temporary corrosion protection. Tribology & Lubrication Technology, 28–34. https://www.stle.org/images/pdf/STLE_ORG/BOK/LS/Metalworking/Fundamentals%20of%20RUST%20PREVENTIVES%20used%20for%20temporary%20corrosion%20protection.pdf
  10. SSPC: The Society for Protective Coatings [SSPC]. (2015). SSPC-SP 1, Solvent cleaning. SSPC, now AMPP.
  11. Wang, J., Severtson, S. J., & Geil, P. H. (2007). Brittle–ductile transitions and the toughening mechanism in paraffin/organo-clay nanocomposites. Materials Science and Engineering: A, 467(1–2), 172–180. https://doi.org/10.1016/j.msea.2007.02.112

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.