KALTECKOREA

BlogApplication notes

Why do rubber parts stick in the mould and tear?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Release & Process Aids

Applying release agent more often and more heavily is the usual response when rubber parts stick in the mould and tear, but if the sticking has another cause, parts stick again and layers of built-up agent tend to foul the mould. What actually lies behind it can be a worn-out release coat, the wrong mould temperature, a tacky compound, incomplete cure or a fouled or worn mould surface, and often two or more at once.

Background

The press opens and the operator pulls on a rubber part, but one end stays stuck to the cavity floor, stretches out and tears. The fragment left in the mould must be scraped out before the next shot, and the next part tends to stick again where it was removed. Torn parts are scrapped, and parts that escape tearing but leave with stretch marks or small, barely visible tears can leak in sealing duties. Time spent prising stuck parts out in front of a hot mould lengthens the cycle and raises the risk of burns.

At the moment a rubber part leaves the mould, two forces compete. One is the rubber's grip on the mould face; the other is the ability of the hot rubber, stretched by that grip, to hold together without tearing. The grip comes from molecular attraction between the two surfaces, chemical bonding, and how far the rubber has pressed into and locked with the fine roughness of the mould face (Awaja et al., 2009). The ability to hold together depends on how many crosslinks, the bonds tying rubber chains to each other, have formed, and tear strength rises as crosslinks increase until it peaks at some intermediate point (Coran, 2005). When the grip grows or the strength falls until the grip wins, the part tears in the mould.

Release agent only lowers the grip; it does nothing for the strength. So if the rubber has not built up enough strength to resist tearing, or the grip has risen for some other reason, adding release agent will not stop the tearing from coming back.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: keep the torn parts and the fragments left in the mould, log which cavity and which spot tore and on which shot, with the mould temperature, cure time and last release agent application at the time, and compare them with the compound's technical data sheet, the TDS, the cure schedule and the release agent's TDS.

Hypothesis 1: worn-out release coat

If parts release well for a while after release agent is applied and then begin to stick as shots accumulate, first ask whether the release coat has worn away. This is especially likely with the first coat after a mould clean, on lines where the reapplication interval is set by the operator's feel rather than by shot count, and in multi-cavity moulds where the rubber strikes different spots with different force. Consider a multi-cavity mould coated in the morning before production starts. From around midday, parts start sticking in the same two or three cavities only, and the torn fragments are always left near the gate where rubber first flows in.

A release coat is a consumable that shrinks with use. Observations in composite moulding show that with every moulding some release coat molecules transfer to the part, thinning the coat left on the mould, and that some cured resin may stay stuck to the mould face on removal (Bainbridge et al., 2021). Where the coat thins first, rubber touches the mould face directly, the grip rises, and that area stretches and tears on removal. One semi-permanent release agent data sheet states that the touch-up interval depends on the material moulded, the mould configuration and abrasion conditions, and advises touching up only where release has worsened (Henkel, 2015). The interval, in other words, is not a single fixed figure but one to be found for that mould and that compound.

Counting, cavity by cavity, the shot at which sticking starts after release agent is applied is the first step. If sticking begins at much the same count each time, that count can be read as the life of the coat. Mark where parts stick on a drawing to see whether it matches the gate or spots where flow strikes hard, and check whether a touch-up on the sticking cavity alone brings clean release at once. Immediate improvement after touch-up strengthens this hypothesis.

If the coat's life is short, move application from operator feel to a shot-count rule. Set the interval well ahead of the count at which sticking begins, and give cavities where flow strikes hard an interval of their own. Touch up thinly and only where release has worsened so that coats do not stack, and keep to the drying and cure times in the TDS. If parts stick again within a few shots of a touch-up, the problem lies less with the coat than with the mould surface or the compound.

Hypothesis 2: mould too hot or cold

The platen temperature set and the actual mould face temperature can differ. Look at this hypothesis when a heater or temperature sensor has failed, when the sensor sits far from the mould face, when the centre and edges of the mould differ, or when preheating is short after a mould change. The same applies when cure temperature has been raised to shorten the cycle. Think of the day after mould temperature was stepped up and cure time cut to raise output: parts are firm and fully cured, yet now tear more easily on removal. Other lines see soft parts tearing only in the first few shots on Monday morning.

Temperature acts in two directions. Too low, and cure slows so that crosslinking falls short within the set time; too high, and the rubber tears more easily as it comes out. In carbon-black-filled rubber, the critical tear energy at which a tear starts to run fell exponentially as temperature rose (Luo et al., 2019). Sulfur-cured isoprene rubbers suffer reversion when cured too long, the breaking of crosslinks already formed, and it is most severe above about 155 °C (Coran, 2005). A study of natural rubber with a conventional sulfur system likewise reports that reversion can appear even at 150 °C if cure is prolonged (Pöschl et al., 2024). A hot mould thus weakens the rubber at removal and, taken too far, also cuts crosslinks, eroding tear resistance twice over.

Measure the mould face directly with a surface thermometer. Take the centre, the edges and the cavities that tear, compare them with the set point, and measure again just after start-up and a few hours later to see how they drift. Check whether the tearing cavities coincide with unusually hot or cold spots, and look at the heater and sensor maintenance records as well. If torn parts are tacky and soft, suspect a cold mould and short cure first; if they are firm and fully cured but began tearing after temperature was raised, suspect tearing while hot.

Putting heaters, sensors and platen contact right comes first; then set a standard preheat time after mould changes. If the aim is to raise temperature to cut time, decide only after reviewing the cure curve measured at that temperature with the compound supplier. If cure is sufficient but parts tear while hot, lower the mould temperature within the TDS range, or blow in air or change the direction of pull on removal so that force does not concentrate at one point.

Hypothesis 3: tacky compound

If sticking began after a compound change, with mould and release agent unchanged, suspect the compound. Typical cases are compounds where plasticiser, oil or tackifying resin was changed or increased, and compounds whose raw material supplier or lot changed. In the first week after the plasticiser type was changed to cut cost, an operator reports that each time the mould opens, parts peel off the mould face with an audible smack and the thin lips tear. A thin, tacky film that comes off on the fingers remains on the mould face.

Tackiness has a name. The tendency of uncured rubber to stick to another surface after brief contact under pressure is called tack, and its size is set by how closely the rubber surface flows into contact with the other face and how far its chains then penetrate and entangle (Hamed, 1981). Before cure begins in the mould, the rubber flows along the mould face and fills its roughness, so a compound that flows easily and is tacky can make wider and deeper contact with the face. Some ingredients also move to the mould face during cure and build up there; in tyre mould tests, zinc sulfide was one of the main contaminants left on the mould face after vulcanisation (Zhang et al., 2022). A film left this way can give the next shot's rubber a foothold.

Line up the compound change history, raw material lots, mixing dates and storage times against the date the trouble began. If old and new compounds can be moulded alternately in the same mould, that is the clearest comparison. Press a finger on uncured rubber and lift it to compare tackiness with a good lot. Wipe the tacky film off the mould face with a clean cloth and record its colour and amount, so that changes after a compound adjustment can be compared.

If the evidence leans towards the compound, review the changed ingredient and its amount with the compound supplier. Consider adjusting the type and amount of plasticiser or tackifying resin, or adding an internal release ingredient or processing aid that helps ejection, checking the compound's cure characteristics and physical properties along the way. Use mixed rubber first in, first out, and mould it within the storage life the compound supplier sets.

Hypothesis 4: incomplete cure

This hypothesis comes up when cure time has been cut, when thick parts are moulded on the same settings as thin ones, or when the weighing of curatives or accelerators has wavered. A cold mould gives the same result, so look at it together with the temperature hypothesis. Take a press that alternates two parts of different thickness on the same cure time. The thin part is fine, but the thick one stretches and tears through the middle on removal, and the torn face is tacky and holds a fingernail mark for a long time.

Cure is the process in which a crosslinking agent such as sulfur bridges the rubber chains, turning rubber that flowed into rubber that springs back after stretching. Stiffness keeps rising as crosslinks increase, but tear strength, fatigue life and toughness peak at an intermediate crosslink density, so a part removed short of crosslinks has not yet built up its resistance to tearing (Coran, 2005). The progress of cure is followed with a cure meter, which twists the rubber slightly at a set temperature and records torque, giving values such as the time for torque to start rising and the time to reach a set fraction of maximum torque (ASTM International, 2019). Heat takes time to reach the middle of a thick section, so the centre can leave the mould under-cured even when the skin is done.

Run the compound on a cure meter at the actual mould face temperature to get the time to a high fraction of maximum torque, and compare it with the current cure time. Compare the hardness of torn and good parts with a durometer, and cut thick parts to measure hardness at the skin and centre separately. If needed, measure tear strength by the standard test method and compare it with fully cured test pieces (ASTM International, 2020). Check the weighing records as well to confirm curatives and accelerators went in at the right amounts.

Correct short cure by resetting the cure time to the measured value and give thick parts their own settings. If more time is hard to find, consider raising the temperature only after checking the cure curve and any reversion at that temperature. An incoming check that runs a cure meter curve on every compound lot and compares it with a reference curve catches lots slowed by weighing or raw material changes before they reach the press.

Hypothesis 5: fouled or worn mould

In moulds left uncleaned for a long time, moulds with layers of fouling, moulds whose plating or coating has worn through, or moulds scratched by coarse abrasives during cleaning, the mould face itself may be the problem. Even within one mould, sticking may recur in particular cavities or spots only. Open a mould run for months without cleaning, and the cavity floor has lost its original shine under a dull film. Rubber sticks and leaves torn fragments wherever the film is thick, and touch-ups of release agent do not last.

A mould face that is smooth and low in surface energy lets go of rubber more readily. In a test comparing six coatings for tyre moulds, the coated faces needed at least 24% less demoulding force than bare steel, smoother surfaces gave lower demoulding force, and surfaces with carbon–fluorine bonds kept less rubber residue (Zhang et al., 2022). The condition of a coating matters too: a PTFE coating with fine cracks released poorly because resin penetrated the cracks under heat and pressure, while a composite plating of fine PTFE particles dispersed in hard nickel was robust enough for industrial use and released well (Critchlow et al., 2006). A fouled or scratched, roughened face offers more places for rubber to key into, and the release coat tends to wear there first.

Open the mould and examine the cavity faces under bright light. Look for dull film, scratches and spots where plating or coating has worn away, and mark whether they match where parts stick and fragments remain. Comparing release just before and just after a clean, with the same compound and release agent, shows how much the surface accounts for. If a roughness tester is available, measure and record roughness at sticking and non-sticking spots.

With the cause narrowed to the mould surface, turn cleaning into scheduled maintenance. Set the cleaning interval in shots and choose a method that does not scratch the mould face. A maker's data sheet states that all prior release agent and soil must be removed before semi-permanent release is reapplied, and that light abrasives can be used on heavy build-up (Henkel, 2015). If scratches or coating damage are severe, review repolishing or a surface treatment such as a fluoropolymer coating or nickel–PTFE composite plating with the mould maker.

Finding the cause

There is no need to dig into all five hypotheses at once. Rule out first what can be checked without stopping the line. Mould face temperature takes a few minutes with a surface thermometer, and the shot count since release agent was applied and the compound change history are in the records. Time-consuming work such as cure meter tests, before-and-after cleaning comparisons and surface analysis comes later.

Next is the pattern of sticking and tearing. If sticking starts at a similar shot count after application and a touch-up cures it at once, look at the life of the release coat; if parts stick again within a few shots of a touch-up, look at the mould surface or the compound. Trouble that recurs only in certain cavities or spots points to temperature and surface at that spot, and trouble that started the day the compound changed points to the compound. Tacky, soft torn faces concentrated in thick parts point to incomplete cure, while tearing in fully cured rubber that began after mould temperature was raised points to tearing on removal from a hot mould.

If the pattern does not settle it, run control trials that change one thing at a time. Compare a freshly cleaned mould with an uncleaned one on the same compound, alternate old and new compound lots, look separately at a few shots with longer cure, and step the mould temperature once. Change only one thing at a time, or there is no telling which change worked.

The figures for judging improvement are torn parts per set number of shots and the number of stops to scrape out fragments. Count them on the same basis as before the change, and measure the parts' tear strength by the standard test method against parts made before the change (ASTM International, 2020). The cause has been removed only once these figures have returned to normal and stayed there over several shifts.

The hypotheses can overlap. On a fouled mould face the release coat wears quickly, touched-up release agent builds up along with the fouling, and a cold mould brings incomplete cure with it. In such cases, clean the mould and bring the mould face temperature into line first, then look again at the release interval and the compound, because while the mould face and temperature are unsettled, the effect of changing release agent or compound cannot be compared fairly.

Limits and cautions

Cure temperature and time, release agent intervals and mould coating choices differ by rubber type, compound and mould, so numeric decisions follow the compound TDS, the release agent TDS and the mould maker's guidance. Tear strength results hold for the conditions of that test and do not translate directly into service performance, so their meaning must be judged product by product (ASTM International, 2020). For sealing or safety-related parts, do not release on floor judgement alone; go through the customer's specified tests and the quality engineer's confirmation.

Safety matters too. Wear heat-resistant gloves when removing parts from a hot mould or cleaning it, and reach into the mould only with the press stopped and locked out. Fume and dust from rubber processing are linked to an increased cancer risk for workers; fit local exhaust ventilation at presses, and keeping rubber no hotter than the process requires can cut fume significantly (HSE, n.d.). Use release agents and mould cleaners with the ventilation and protective equipment set out in each product's safety data sheet, the SDS.

Sources

  1. ASTM International. (2019). ASTM D5289-19a, Standard test method for rubber property—Vulcanization using rotorless cure meters. https://store.astm.org/d5289-19a.html
  2. ASTM International. (2020). ASTM D624-00(2020), Standard test method for tear strength of conventional vulcanized rubber and thermoplastic elastomers. https://store.astm.org/d0624-00r20.html
  3. Awaja, F., Gilbert, M., Kelly, G., Fox, B., & Pigram, P. J. (2009). Adhesion of polymers. Progress in Polymer Science, 34(9), 948–968. https://doi.org/10.1016/j.progpolymsci.2009.04.007
  4. Bainbridge, K., Schoenholz, C., & Zobeiry, N. (2021). Investigating the aging of release coating in aerospace composites manufacturing. Undergraduate Research in MSE, 2. https://doi.org/10.6069/ssywg443
  5. Coran, A. Y. (2005). Vulcanization. In J. E. Mark, B. Erman, & F. R. Eirich (Eds.), Science and technology of rubber (3rd ed., pp. 321–366). Elsevier Academic Press. https://doi.org/10.1016/B978-012464786-2/50010-9
  6. Critchlow, G. W., Litchfield, R. E., Sutherland, I., Grandy, D. B., & Wilson, S. (2006). A review and comparative study of release coatings for optimised abhesion in resin transfer moulding applications. International Journal of Adhesion and Adhesives, 26(8), 577–599. https://doi.org/10.1016/j.ijadhadh.2005.09.003
  7. Hamed, G. R. (1981). Tack and green strength of elastomeric materials. Rubber Chemistry and Technology, 54(3), 576–595. https://doi.org/10.5254/1.3535821
  8. Health and Safety Executive [HSE]. (n.d.). Safe to breathe: Dust and fume control in the rubber industry. Retrieved November 2026. https://www.hse.gov.uk/pubns/iacl95.htm
  9. Henkel. (2015). Technical data sheet: LOCTITE FREKOTE 44-NC. Henkel Corporation.
  10. Luo, W., Li, M., Huang, Y., Yin, B., & Hu, X. (2019). Effect of temperature on the tear fracture and fatigue life of carbon-black-filled rubber. Polymers, 11(5), 768. https://doi.org/10.3390/polym11050768
  11. Pöschl, M., Sathi, S. G., & Stoček, R. (2024). A chemical interpretation for the post-reversion upturn in the natural rubber/accelerated sulfur system based on the viscoelastic properties and cross-link density measurements. Polymer Bulletin, 81(14), 12521–12541. https://doi.org/10.1007/s00289-024-05292-z
  12. Zhang, X., Liu, Z., Wang, X., Xu, X., Wu, Y., & Wu, D. (2022). Comparative study of anti-sticking properties of coatings for tire molds. Coatings, 12(11), 1740. https://doi.org/10.3390/coatings12111740

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.