Blaming the scratch and touching up just that spot is the usual response to rust spreading from a scratch, but how fast rust creeps under the paint depends heavily on the interface around the scratch and the water and salt reaching it, so covering the surface alone tends to let it spread again. What actually lies behind it can be poor surface preparation, a thin film, salt left on the steel, a weak inhibitive primer, or salty, damp service, and sometimes two or more at once.

Background

Coated steelwork gets scratched in transport or assembly. At first it is one fine line, but a few months later a band of brown rust has spread along it, and the paint beyond the band looks sound yet lifts away in wide flakes when pushed with a knife point. Once the lifted paint is stripped for repair, the area to clear turns out far larger than the rust first seen, and appearance claims and repainting costs grow together. On a structure, corrosion running under the paint can eat into the steel section itself.

At a scratch the steel is bare, and once water and salt reach it, iron starts to dissolve there. The scratch becomes the anode that gives up electrons, and the interface under the paint just around it becomes the cathode, where oxygen from the air takes up electrons and is reduced. Oxygen reduction makes the interface strongly alkaline, and that alkali, together with reactive species formed along the way, breaks the bond between paint and metal so the paint lifts further in. This is called cathodic delamination, and it is described as the main path by which disbonding runs under the paint from a defect (Leidheiser et al., 1983; Grundmeier et al., 2000).

So how fast rust spreads depends not only on the scratch itself but heavily on the state of the interface around it and on how often water and salt reach it. That is why scratches made on the same day can show different creep widths from part to part and from place to place.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: measure and log how far rust and lifting have spread from the scratch, and compare the painting specification, the paint's technical data sheet, the TDS, and the records of surface preparation grade, film thickness and application conditions at the time. Standard methods exist for measuring delamination and rust width around a scribe on test panels, and they can anchor judgement on site too (ISO, 2012b; ASTM International, 2024).

Hypothesis 1: poor surface prep

This hypothesis comes up first when loose rust was only brushed off by hand or power tool instead of blast cleaning, when paint went straight onto steel still carrying mill scale, the black iron oxide skin from rolling, when it went over oil, or when a conversion coating step such as phosphating was skipped. It readily causes trouble in site repair painting and on lines where small parts are painted by hand. Think of a railing on a repair job. Loose rust was brushed off and new paint went straight over it, and for a while it looked fine. Rust then started spreading along a scratch made while a bolt was retightened, and when the paint around the scratch was lifted with a knife point, wide pieces came away easily with black flakes stuck to their backs.

How well paint holds around a scratch depends on what it is stuck to. The protective power of a coating rests heavily on the bond at the metal–paint interface and the state of the oxide beneath it, and delamination advances along exactly that interface (Grundmeier et al., 2000). Paint applied over scale, rust or oil is attached to that weak layer rather than to the steel, so water and alkali entering at the scratch work their way along it easily. Surface shape plays a part too. In tests of an epoxy on abrasive-blasted steel, the cathodic delamination rate depended on how fast ions moved along the interface from the defect to the delamination front, so surface topography had a strong effect, and the authors judged that blasting could lower the delamination rate to some extent (Sørensen et al., 2009b). A phosphate conversion coating is likewise a layer applied before painting to raise adhesion and corrosion resistance (Narayanan, 2005).

Checking begins by stripping a little paint beyond the end of the creep and looking at the surface underneath. Black scale, red rust or smooth, shiny rolled surface means preparation fell short. Rust grades and preparation grades are defined by reference photographs, so compare what is left with those photographs and with the grade in the application records (ISO, 2007). Note what is stuck to the back of the lifted paint, and whether paint on an area with no creep also comes away easily when tape is pressed over a knife-cut X and pulled off.

With the cause narrowed to surface preparation, strip the lifted paint beyond the end of the rust, re-prepare to the grade the specification calls for, then paint. Switch to blast cleaning for parts that allow it, and feather the edges of the old paint around repairs so the new coat joins smoothly. On a conversion coating line, review the control items of that step first. From the next job on, add a step that compares the surface with the reference photographs before painting.

Hypothesis 2: thin film

Film tends to end up thinner than specified on repairs finished with a single brush or roller coat, when paint was heavily thinned, when the spray gun was held too far off, and on faces the operator reached less, such as the back of a complex shape. All the more so on lines that pass parts on by colour alone without measuring thickness. Take a bundle of small brackets finished in a single coat. Several picked up similar scratches during unpacking, and a few weeks later the width of rust around the scratches varies from one part to the next.

Organic coatings do not stop water, oxygen and ions completely; they let them through slowly. Barrier protection works by slowing that passage, and the path grows longer with thicker films and more coats. So the standard for selecting paint systems sets the system build-up and film thickness by the corrosivity category of the environment and the expected durability (Sørensen et al., 2009a; ISO, 2019). A blasted surface has peaks and valleys, with the thinnest film over the peaks, and readings taken on a rough surface differ from the true thickness, so there is a separate method and acceptance criteria for measuring dry film thickness on rough surfaces (ISO, 2012a). In tests that measured cathodic delamination from a defect, however, epoxy film thickness had little influence while surface topography had a large one (Sørensen et al., 2009b). A thin film weakens protection overall, but thickness alone rarely explains how fast rust creeps around a scratch.

Measure first. Read the dry film thickness around a scratch with creep and in an area without it using the same method, correct the readings as the rough-surface standard describes, and compare them with the specified thickness. Magnifying a cross-section of the scratch, or cutting the paint at a shallow angle, shows the number of coats and the thickness of each, which reveals whether a primer was left out or only the topcoat is thick. Record which faces of the shape are thin and whether the rust is concentrated on them.

Once the film is shown to fall short of the specification, make thickness measurement a formal step in application, and bring the thinning ratio and application method back within the TDS. Paint hard-to-reach faces separately first, and build repairs up with the number of coats in the specification. If the film meets the specification and rust still spreads, weigh causes at the interface and in the environment more heavily than thickness.

Hypothesis 3: salt left on steel

Suspect salt on steel stored for a long time in a coastal yard, on parts hauled along roads splashed with winter de-icing salt, when repainting steel that had deep rust pits, and when paint went on some time after blasting at a site exposed to sea wind. Salt cannot be seen, so it can remain even when the surface looks an even clean grey. Say steel that spent several months in a coastal yard was blasted and painted. Before painting the surface was an even grey, and the film met its thickness. About a year later, small blisters rise in a row along with rust around a scratch.

When water-soluble salts such as chlorides or sulfates stay under the paint, water slowly passing through the film is drawn to them. Osmosis, water moving towards the higher salt concentration, raises blisters, and the concentrated brine trapped beneath speeds up corrosion (Morcillo, 2003). Salt also acts on delamination around a scratch. In a study that tracked delamination on steel, it advanced as cations from the defect moved along the interface to the delamination front, and the higher the cation concentration at the defect, the faster it went (Leng et al., 1999). By that result, salt already lying at the interface can work by supplying ions to the delamination front in advance. Salt at the bottom of deep rust pits may not all come out with blasting, and methods have been set out for dissolving salts off the surface with water and analysing them (FHWA, 2014).

Salt shows only when measured. On surfaces still to be painted, test after blasting and before painting; where creep has already happened, test on the surface exposed by stripping the paint. Dissolve the salt from a set area with water and estimate its amount from the electrical conductivity of that water; this field conductivity method is set out in a standard (ISO, 2020). Record whether blisters accompany the creep and what the liquid inside looks like when one is opened, and check where and for how long the steel was stored.

If salt appears to remain, wash it off with clean water at high pressure before repainting, blast again, then measure to confirm it is within the limit before painting. The allowable salt level follows the painting specification and the paint supplier's guidance; write that limit and the measuring step plainly into the specification. Store steel that passes through coastal or de-icing salt areas under cover, and shorten the time between blasting and painting.

Hypothesis 4: weak inhibitive primer

Look at this hypothesis when the primer was changed to another product for cost, when the topcoat went straight onto steel with no primer, when a general-purpose undercoat without inhibitive pigment was used, or when a zinc-dust primer went on too thin. It can arise when paint from a different supplier comes in on an extension project. Consider a plant where a section added later, painted with another supplier's primer, sits right next to the original section. Both got scratched over the same winter, but on one side the scratch stayed a thin line of rust while on the other the rust spread wide.

Anticorrosive paints protect steel in three ways: a barrier that blocks the path of water and oxygen, inhibition, where pigment dissolves out and suppresses reactions on exposed steel, and sacrificial protection, where zinc corrodes in place of the steel (Sørensen et al., 2009a). At a scratch the barrier is gone, so slowing creep from it falls to the other two. Zinc phosphate was proposed as a non-polluting replacement for lead and hexavalent chromium pigments and is widely used, but how it protects is still not fully explained (Romagnoli & Vetere, 1995). For zinc-dust primers there is a five-year offshore field test. Systems with zinc silicate primers all performed well, while zinc epoxy primers gave varied results, which the authors thought the primer film thickness had probably affected. A system with epoxy mastic applied straight onto blasted steel, with no zinc primer, also performed reasonably well (Knudsen et al., 2005). In other words, whether the primer went on at its proper thickness matters as much as its type.

Start by confirming from the records and the TDS which primer actually went on. Check the composition section of the safety data sheet, the SDS, for inhibitive ingredients such as zinc dust or zinc phosphate, and measure in a scratch cross-section or an angled cut whether a primer coat is present and whether its thickness is within the TDS range. If the site has sections with different primers, compare creep widths section by section.

If the primer is to blame, go back to the inhibitive primer type named in the specification, starting with the most corrosive locations, and keep zinc primers within the TDS thickness range. Before adopting a substitute primer, make test panels on the same steel with the same preparation, scribe them deliberately, measure creep width around the scribe by a standard method, and compare it with the existing product before deciding.

Hypothesis 5: salt and moisture

This hypothesis covers coastal plant, structures along roads spread with de-icing salt, indoor areas near food or plating plants where wash water and condensation keep returning, and spots where water pools on flat faces or that keep wetting and drying. It applies especially when the paint system is the same and only the location differs. The same part, painted to the same specification, hangs indoors under a roof in one place and outdoors facing the sea in another. Both were scratched during installation, and a year later the scratches on the outdoor part are covered in wide rust bands, wider still on the underside and on ledges where water collects.

For corrosion to continue from a scratch, the scratch and its surroundings must be linked by water, and salt turns that water into an electrolyte that conducts well. The corrosivity category of an atmosphere is rated from the first-year corrosion of standard specimens, or estimated from environmental values such as temperature, humidity, sulfur dioxide and airborne salinity (ISO, 2012c). On the delamination side, the study cited earlier found that the type of anion did not much affect the rate, while the type and concentration of cations changed it, and that early on the delaminated area grew in proportion to time (Leng et al., 1999). Where salt arrives often and surfaces stay wet long, cations keep reaching the scratch, so delamination can carry on without stopping. This is also why a higher corrosivity category calls for a different paint system and film thickness (ISO, 2019).

Start by mapping the creeping scratches by location. See whether they cluster on faces towards the sea or road, on undersides, on ledges where water pools or where wash water splashes, and compare creep widths with indoor parts of the same specification. Sampling salt from suspect surfaces and measuring its conductivity gives an estimate of how much salt is building up from outside. Check in the specification which corrosivity category was assumed for the site at design, and if needed hang standard specimens and re-rate the category from one year's corrosion.

If the environment proves harsher than the specification assumed, reset the repair specification to a paint system for that category. Drill drain holes or change the shape where ledges hold water, and add regular fresh-water washing of salt-collecting spots to the inspection list. The sooner a new scratch is repaired before rust spreads, the less paint has to be stripped, so set a short inspection interval for scratches.

Finding the cause

There is no need to investigate all five hypotheses at once. Rule them out starting with what can be seen without breaking the paint. Film thickness can be read straight away with a gauge, primer type and preparation grade are in the records, and the pattern of creep can be logged by walking the site. Salt on the surface and the surface under the paint can only be seen once paint is stripped, so they come next.

The shape of the creep is a strong clue. Rust concentrated on faces towards the sea or road, on undersides or where water pools points first to salty, damp service. Wide creep across a whole lot or section, regardless of position, points to surface preparation or primer, which affect the whole process; blisters rising in rows along with the rust point to salt left on the steel. Scale or rust stuck to the back of lifted paint points to surface preparation.

If that still does not settle it, make control panels. On the same steel, change only the surface preparation, or only the primer, or only the film thickness, scribe each with the same mark, and hang them in the same place. Change only one thing at a time, or there is no telling which made the difference. Measure delamination and rust width around the scribe by the standard method, so that panels and dates can be compared (ISO, 2012b).

The final check is made at the repaired areas. After correcting the cause and repairing, measure and log the creep width of new scratches by the same method at fixed intervals. The cause has been found only when creep in the same environment is clearly smaller than before. Test panel results and site results can differ, so site records are the basis for the final judgement.

The hypotheses can overlap. A surface with residual salt causes more trouble in a damp environment, and where a thin film and a weak primer come together, rust tends to spread faster from a scratch. In such cases, correct surface preparation and residual salt first. Those two cannot be fixed without stripping once paint is on, whereas film thickness, primer and environmental care can be dealt with at the next painting or inspection.

Limits and cautions

Surface preparation grade, film thickness, allowable salt level and paint system build-up vary with environment and paint, so numeric decisions follow the painting specification and the TDS of the paint in question. Accelerated test results may not match service life directly, so decisions to change products are made together with site records. On safety-related structures such as bridges, tanks or pressure equipment, if corrosion has spread widely under the paint, have a coatings specialist and the structural engineer assess the loss of steel section.

Safety matters too. For blasting dust, solvents in paints and thinners, and zinc dust, follow the product SDS for protective equipment and ventilation, and in confined spaces such as tank interiors follow the set entry procedure. Before stripping old paint, check whether it contains hazardous ingredients, and remove and dispose of it by a suitable method.

Sources

  1. ASTM International. (2024). ASTM D1654-24, Standard test method for evaluation of painted or coated specimens subjected to corrosive environments. https://store.astm.org/d1654-24.html
  2. Federal Highway Administration [FHWA]. (2014). Methodology for analysis of soluble salts from steel substrates (FHWA-HRT-14-026). U.S. Department of Transportation. https://www.fhwa.dot.gov/publications/research/infrastructure/structures/bridge/14026/index.cfm
  3. Grundmeier, G., Schmidt, W., & Stratmann, M. (2000). Corrosion protection by organic coatings: Electrochemical mechanism and novel methods of investigation. Electrochimica Acta, 45(15–16), 2515–2533. https://doi.org/10.1016/S0013-4686(00)00348-0
  4. International Organization for Standardization [ISO]. (2007). ISO 8501-1:2007, Preparation of steel substrates before application of paints and related products — Visual assessment of surface cleanliness — Part 1: Rust grades and preparation grades of uncoated steel substrates and of steel substrates after overall removal of previous coatings. https://www.iso.org/standard/43426.html
  5. International Organization for Standardization [ISO]. (2012a). ISO 19840:2012, Paints and varnishes — Corrosion protection of steel structures by protective paint systems — Measurement of, and acceptance criteria for, the thickness of dry films on rough surfaces.
  6. International Organization for Standardization [ISO]. (2012b). ISO 4628-8:2012, Paints and varnishes — Evaluation of degradation of coatings — Designation of quantity and size of defects, and of intensity of uniform changes in appearance — Part 8: Assessment of degree of delamination and corrosion around a scribe or other artificial defect. https://www.iso.org/standard/51942.html
  7. International Organization for Standardization [ISO]. (2012c). ISO 9223:2012, Corrosion of metals and alloys — Corrosivity of atmospheres — Classification, determination and estimation. https://www.iso.org/standard/53499.html
  8. International Organization for Standardization [ISO]. (2019). ISO 12944-5:2019, Paints and varnishes — Corrosion protection of steel structures by protective paint systems — Part 5: Protective paint systems. https://www.iso.org/standard/77795.html
  9. International Organization for Standardization [ISO]. (2020). ISO 8502-9:2020, Preparation of steel substrates before application of paints and related products — Tests for the assessment of surface cleanliness — Part 9: Field method for the conductometric determination of water-soluble salts.
  10. Knudsen, O. Ø., Steinsmo, U., & Bjordal, M. (2005). Zinc-rich primers—Test performance and electrochemical properties. Progress in Organic Coatings, 54(3), 224–229. https://doi.org/10.1016/j.porgcoat.2005.06.009
  11. Leidheiser, H., Jr., Wang, W., & Igetoft, L. (1983). The mechanism for the cathodic delamination of organic coatings from a metal surface. Progress in Organic Coatings, 11(1), 19–40. https://doi.org/10.1016/0033-0655(83)80002-8
  12. Leng, A., Streckel, H., & Stratmann, M. (1999). The delamination of polymeric coatings from steel. Part 2: First stage of delamination, effect of type and concentration of cations on delamination, chemical analysis of the interface. Corrosion Science, 41(3), 579–597.
  13. Morcillo, M. (2003). Soluble salts: Their incidence on the protection of metallic structures by paint coatings. Revista de Metalurgia, 39(Extra), 219–227. https://doi.org/10.3989/revmetalm.2003.v39.iExtra.1123
  14. Narayanan, T. S. N. S. (2005). Surface pretreatment by phosphate conversion coatings – A review. Reviews on Advanced Materials Science, 9, 130–177. https://ipme.ru/e-journals/RAMS/no_2905/narayanan.html
  15. Romagnoli, R., & Vetere, V. F. (1995). Non-pollutant corrosion inhibitive pigments: Zinc phosphate, a review. Corrosion Reviews, 13(1), 45. https://doi.org/10.1515/CORRREV.1995.13.1.45
  16. Sørensen, P. A., Kiil, S., Dam-Johansen, K., & Weinell, C. E. (2009a). Anticorrosive coatings: A review. Journal of Coatings Technology and Research, 6(2), 135–176. https://doi.org/10.1007/s11998-008-9144-2
  17. Sørensen, P. A., Kiil, S., Dam-Johansen, K., & Weinell, C. E. (2009b). Influence of substrate topography on cathodic delamination of anticorrosive coatings. Progress in Organic Coatings, 64(2–3), 142–149. https://doi.org/10.1016/j.porgcoat.2008.08.027

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.