Switching to a product labelled oil-resistant or chemical-resistant is the usual response when sealant swells and softens, but which liquids a sealant withstands depends on its polymer, so choosing by the label alone tends to repeat the problem. What actually lies behind it can be a polymer that does not suit the liquid, plasticiser leaving the sealant, high temperature or cleaning chemicals, and sometimes two or more at once.

Background

Around pump bases, on tank manhole rims and along machine cover joints, sealant bulges out of the joint within weeks. A finger presses into it more easily than before, the surface is tacky, and a knife cut shows it soft right through. Given more time, the swollen sealant lifts from the bonded faces or tears through the middle, and oil and chemicals seep out through the gap.

When sealant gives way, the liquid it was meant to hold back comes out. Oil spread on the floor becomes a slip and fire hazard, and a chemical leak leads on to equipment corrosion and environmental trouble. Resealing means stopping the equipment, scraping out the softened sealant and cleaning the faces again, so reapplying the same product without knowing the cause only repeats the cost.

Cured sealant is a rubber in which polymer chains are linked into a network. When liquid molecules seep into that network, the volume grows; this is swelling. The more liquid enters, the more the stretched network pulls back, and swelling stops where the pull of the liquid and the pull of the network balance, so a more tightly linked network swells less (Flory & Rehner, 1943). How much enters depends on how chemically alike the liquid and the polymer are, and the solubility parameter is the number that expresses this likeness. The closer the values, the more the liquid swells the polymer (Hansen, 2007).

The liquid that enters pushes the chains apart and lets them slide past one another, so the sealant softens and loses strength as it swells. At the same time the liquid can draw out components of the sealant that dissolve in it. That is why the standard test for how rubber withstands liquids measures changes in mass, volume, hardness and tensile strength before and after immersion, along with the amount of soluble matter the liquid extracts (ASTM International, 2021).

In such cases the technical team sets up the four hypotheses below and rules them out one by one. The start is always the same: identify exactly which liquids reach the sealant and what they contain from their safety data sheets, the SDS, note the contact temperature and the way they reach it, whether constantly immersed, splashed and left to dry, or only as vapour, and compare all this with the chemical resistance data in the sealant's technical data sheet, the TDS.

Hypothesis 1: wrong polymer

This hypothesis comes to mind first when a sealant made for building or general use goes around machinery that oil reaches. The same applies after the fuel is switched to a biodiesel blend or an alcohol blend, or after equipment is moved next to a process that uses solvents. Picture a pipe penetration beside a hydraulic unit, closed with a general-purpose silicone. Months later only the lower side, where oil beads, has bulged and takes a fingernail easily, while the upper side that oil never reaches looks as it did on the day it was applied.

How far a sealant swells is set not by the polymer alone but by the pairing of polymer and liquid. The base polymer of silicone swelled strongly in hydrocarbons such as hexane and toluene, and the degree of swelling tracked the liquid's solubility parameter (Lee et al., 2003). Nitrile rubber swells more in fuel that contains aromatics, and more still the stronger the polarity and hydrogen bonding of the added aromatic (Graham et al., 2006). Polysulfide and polythioether sealants made for fuel tanks also grew sharply in volume as the aromatic content of the fuel rose (Chen et al., 2013).

In tests in biodiesel and diesel, nitrile and chloroprene rubber degraded more and fluorocarbon rubber was the least attacked (Haseeb et al., 2010). Mineral oils, synthetic oils and fuels blended from plant feedstocks all count as oil, yet their components differ, so a sealant that held up in one cannot be assumed to hold up in another. This is why the single word oil-resistant does not hold for every oil and fuel.

Begin by finding aromatics, alcohols, esters, ketones and similar components in the SDS of the liquid, and confirm the polymer type of the sealant from its TDS. Then measure hardness with a rubber durometer on the side the liquid reaches and on the side it does not. If the difference is clear, immersing leftover sealant or a fresh specimen in that liquid and measuring volume, mass and hardness changes by the standard method shows in numbers whether the pairing works (ASTM International, 2021).

When the pairing proves wrong, change the polymer first. Moving up a grade within the same polymer is often not enough, so choose a product whose TDS or supplier data shows results in the very liquid it will meet. For fuel, look among the polysulfide, polythioether and fluorinated families developed for fuel service, and check the pairing again whenever the fuel or solvent composition changes.

Hypothesis 2: plasticiser loss

Suspect plasticiser where sealant is wetted and dried over and over: around fuelling equipment where fuel or oil splashes and evaporates, in floor joints that are dried after washing, and on equipment that cycles between running and standing. Watch closely, too, right after a switch to a fuel with fewer aromatics. A floor joint in front of a fuel dispenser looks soft and swollen on a day when fuel was spilled. Seen again after a few dry days, though, the sealant has shrunk, a hairline gap has opened at its edge, and the surface has hardened and crazed.

A plasticiser is a small molecule that sits between the chains and softens the sealant; it is not chemically bound to the chains, so it can move out into a liquid in contact (Wypych, 2017). In contact with a liquid, two things happen together: liquid comes in and plasticiser goes out. When more comes in than goes out, the sealant looks swollen and soft while wet, but once the liquid evaporates it shrinks and stiffens by the amount of plasticiser lost. In a study that immersed rubbers for four weeks in test fuels blending gasoline and alcohol, every material swelled while wet, and after drying the nitrile and neoprene shrank and became brittle, which the authors linked to plasticiser extraction (Kass et al., 2014). A change in fuel composition can do the same: a polysulfide sealant immersed in jet fuel with less than 8% aromatics did not swell but lost volume (Chen et al., 2013).

This hypothesis cannot be settled by looking at the wet state alone. Inspect the same spot both when wet and after it has dried thoroughly, and record whether it has shrunk and hardened after drying and whether a gap has opened at the edge. To confirm with a specimen, weigh it before immersion, straight after immersion and again after it has been taken out and dried. If the dried weight is below the starting weight, something has left, and the standard test includes a separate procedure for measuring the soluble matter the liquid extracted (ASTM International, 2021).

If plasticiser appears to be leaving, look for a formulation with little plasticiser or one that is hard to extract. Where joints are wetted and dried, choose a product tested under the same condition, measured after immersion and drying, and ask the supplier for mass loss data in that liquid. When the fuel is changed, put the sealant joints on the inspection list and watch for shrinkage and gaps for several weeks afterwards.

Hypothesis 3: high temperature

Look at temperature where sealant sits with hot liquid: engine compartments, near exhausts, around pipework and heat exchangers carrying hot oil, on heated tanks and on tank roofs under midsummer sun. In one plant, with the same product and the same oil, the joint beside a pump running at room temperature is fine, while only the joint beside the return line carrying hot oil back has swollen and turned tacky. Both joints were applied on the same day by the same worker.

Liquid enters a polymer by diffusion, with molecules working their way between the chains, and diffusion speeds up as temperature rises (George & Thomas, 2001). More liquid gets in, and deeper, in the same time, so a pairing that only swells the surface slightly at room temperature softens right through in a hot spot. This is why laboratories deliberately test hot: the standard test for sealant durability under continuous immersion speeds up deterioration with hot liquid, and states that it predicts long-term durability only when the service temperature is well below the test temperature (ASTM International, 2020). The studies cited above likewise measured swelling and shrinkage at raised temperatures, such as 28 days at 93°C and four weeks at 60°C (Chen et al., 2013; Kass et al., 2014).

Measure the surface temperature where the symptom appears with a contact thermometer or a thermal camera, and find the liquid's peak temperature in the operating records. Compare these with the service temperature range in the TDS and with the temperature at which the chemical resistance data were obtained. If the data come only from room-temperature tests while the real spot runs much hotter, this hypothesis is strong. Measuring hardness at both the hot and the cool spot leaves the difference on record as numbers.

Once the cause narrows to temperature, act in two directions. One is to switch to a product with test data in that liquid at the actual peak temperature; the other is to reduce the heat the sealant receives. Review with the design engineer whether a heat shield or insulation can be fitted, or the joint moved away from the hot surface. Where neither change is practical, shorten the inspection interval and replace the sealant as soon as it starts to swell.

Hypothesis 4: cleaning chemicals

The liquids that reach sealant are not only process liquids. Where equipment is cleaned on a schedule, as in food, pharmaceutical and machinery plants, degreasing solvents, alkaline detergents, sanitisers, high-pressure hot water and steam may reach the sealant more often, and hotter, than the process liquid does. Suspect this hypothesis when an equipment joint that withstood the process oil for years turns tacky and comes off on the hand within months of a switch to a new cleaner.

A cleaner can damage sealant in two ways. Solvents in the cleaner act by the swelling principle above; hydrocarbon degreasers are the typical case, and the base polymer of silicone swelled strongly in solvents such as toluene and hexane (Lee et al., 2003). Each wash may be short, but repeated daily it swells and dries the sealant again and again. Alkaline detergents and hot water take another route. Polyurethanes built on a polyester backbone carry ester links in their chains, and these undergo hydrolysis, breaking on reaction with water. That is why polyester-based polyurethanes are more vulnerable to hydrolysis than those built on a polyether (Xie et al., 2019). Broken chains leave a looser network and the sealant softens, but unlike swelling it does not recover when the liquid evaporates. Polyurethane specimens also degraded in test fuels containing alcohol, so cleaners and sanitisers that contain alcohol belong on the list as well (Kass et al., 2014).

Pull out the cleaning procedure first. Note the chemicals used and their concentration, the cleaning temperature, contact time and whether a rinse follows, and set the date the cleaner or procedure changed against when the symptom first appeared. Measure hardness straight after cleaning and again after at least a day of drying: recovery after drying points to swelling by solvent, while a surface still tacky and soft after drying points to chemical degradation with broken chains. The standard immersion test for sealants does not include acids or alkalis in its basic form, and allows the test liquid to be changed by agreement between the parties, so testing in the actual cleaner can be commissioned (ASTM International, 2020).

If cleaning chemicals are to blame, set the cleaner supplier's data against the sealant supplier's and choose a sealant tested in that cleaner at that temperature. Keep to the cleaner's recommended concentration and temperature, never skip the rinse, and when changing cleaners, immerse a small specimen first before bringing the new one in. If the cleaning cannot change, the remaining route is a sealant polymer suited to those cleaning conditions.

Finding the cause

The four hypotheses need not all be tested at once. Rule out first what documents and a thermometer can confirm. The composition of the liquids and the polymer type of the sealant are in the SDS and TDS, cleaning chemicals and procedures are in the cleaning procedure, and temperature is in the operating records and on the thermometer. Hardness can be measured on the spot, while immersion tests on specimens take time and come last.

The shape of the symptom narrows the cause a great deal. If only the side the liquid reaches swells and softens, and it returns nearly to normal on drying, look first at swelling from a polymer that does not suit the liquid. If it swells when wet but shrinks and hardens on drying, opening at the edge, suspect plasticiser leaving; if the same liquid swells it only at the hot spot, suspect temperature. If it stays tacky and soft after drying, or the trouble began after a change in cleaning procedure, look at the cleaning chemicals.

If that still does not settle it, run control tests. Immerse specimens of the same sealant separately in the process liquid and in the cleaner, at room temperature and at the actual operating temperature, measure volume, mass and hardness, and measure again after taking them out and drying them. Putting candidate sealants side by side under the same conditions selects the replacement at the same time. Accelerated laboratory tests may not correlate directly with real part performance, though, so use the results as a basis for comparison on site (ASTM International, 2021).

The final check happens on site. Apply the new sealant in the same place and, for the first few weeks, measure its hardness and shape at set intervals, comparing them with the records from before the change. The cause can be considered found only when swelling, tackiness and edge gaps do not return and hardness holds steady.

The hypotheses often overlap. Hot fuel increases both swelling and plasticiser extraction, and a cleaner containing solvent swells the sealant while drawing out plasticiser. In such cases, choosing a polymer that suits the liquid and the temperature comes first, because with the wrong polymer, lowering the temperature or changing the cleaning does little, and only once the polymer is right can the effect of changing temperature and cleaning conditions be compared fairly.

Limits and cautions

The chemical resistance of a sealant varies between formulations even within one polymer, so which liquids it can meet and up to what temperature follows the product's TDS and the supplier's test data. Where specifications and approvals apply, as in aircraft and vehicle fuel systems, pressurised tanks, and places in contact with food or drinking water, do not change products on site judgement alone; get confirmation against the relevant specification and from the design engineer.

Safety matters too. Fuels and solvents ignite easily and their vapours can be harmful to breathe, so follow each liquid's SDS for ventilation, control of ignition sources, protective gloves and eye protection. When removing softened sealant, the liquid soaked into it can run out, so have a container ready to catch it, and dispose of the removed sealant and wiping cloths as waste appropriate to that liquid.

Sources

  1. ASTM International. (2020). ASTM C1247-20, Standard test method for durability of sealants exposed to continuous immersion in liquids. https://store.astm.org/c1247-20.html
  2. ASTM International. (2021). ASTM D471-16a(2021), Standard test method for rubber property—Effect of liquids. https://doi.org/10.1520/D0471-16AR21
  3. Chen, K., Liu, H., & Xia, Z. (2013). The impacts of aromatic contents in aviation jet fuel on the volume swell of the aircraft fuel tank sealants. SAE International Journal of Aerospace, 6(1), 350–354. https://doi.org/10.4271/2013-01-9001
  4. Flory, P. J., & Rehner, J. (1943). Statistical mechanics of cross-linked polymer networks II. Swelling. The Journal of Chemical Physics, 11(11), 521–526. https://doi.org/10.1063/1.1723792
  5. George, S. C., & Thomas, S. (2001). Transport phenomena through polymeric systems. Progress in Polymer Science, 26(6), 985–1017. https://doi.org/10.1016/S0079-6700(00)00036-8
  6. Graham, J. L., Striebich, R. C., Myers, K. J., Minus, D. K., & Harrison, W. E. (2006). Swelling of nitrile rubber by selected aromatics blended in a synthetic jet fuel. Energy & Fuels, 20(2), 759–765. https://doi.org/10.1021/ef050191x
  7. Hansen, C. M. (2007). Hansen solubility parameters: A user's handbook (2nd ed.). CRC Press.
  8. Haseeb, A. S. M. A., Masjuki, H. H., Siang, C. T., & Fazal, M. A. (2010). Compatibility of elastomers in palm biodiesel. Renewable Energy, 35(10), 2356–2361. https://doi.org/10.1016/j.renene.2010.03.011
  9. Kass, M. D., Theiss, T., Pawel, S., Baustian, J., Wolf, L., Koch, W., & Janke, C. (2014). Compatibility assessment of elastomer materials to test fuels representing gasoline blends containing ethanol and isobutanol. SAE International Journal of Fuels and Lubricants, 7(2), 445–456. https://doi.org/10.4271/2014-01-1462
  10. Lee, J. N., Park, C., & Whitesides, G. M. (2003). Solvent compatibility of poly(dimethylsiloxane)-based microfluidic devices. Analytical Chemistry, 75(23), 6544–6554. https://doi.org/10.1021/ac0346712
  11. Wypych, G. (Ed.). (2017). Handbook of plasticizers (3rd ed.). ChemTec Publishing.
  12. Xie, F., Zhang, T., Bryant, P., Kurusingal, V., Colwell, J. M., & Laycock, B. (2019). Degradation and stabilization of polyurethane elastomers. Progress in Polymer Science, 90, 211–268. https://doi.org/10.1016/j.progpolymsci.2018.12.003

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.