Why does sealant stay soft where it touches other sealants or gaskets?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Sealants & Damping

Suspecting a bad batch and refilling with the same product is the usual response to sealant that stays soft only where it touches something, but if the neighbouring material stays, the new sealant can go soft in the same place again. What actually lies behind it can be another sealant in contact with silicone, components passing between the sealant and bitumen or butyl, plasticiser from EPDM gaskets, old sealant left behind, or backer rod or solvent used wrongly, and sometimes two or more at once.

Background

A few days after a window frame or panel joint was resealed, most of the bead feels firm, yet the side touching old sealant or a rubber gasket smears on the fingertip and keeps a fingernail mark. That area lifts easily from the substrate, picks up dirt and changes colour, and in the end becomes a path for water. Cutting it out and refilling takes more work than the first job, and in structural glazing, where sealant holds the glass, the bond is the structure, so the problem becomes one of safety (ASTM International, 2023a).

Whether two materials can be used together is a question of compatibility: the ability of each material to keep its usual physical and chemical properties while in contact with or close to the other, and some sealant selection problems come from incompatibility with substrates, primers and other sealants (Persily, 1993). Components do not move only between materials that touch. Materials seek equilibrium and can spread through the whole joint, and heat and ultraviolet light also bear on the outcome (FGIA & NGA, 2023).

So softness only where the sealant touches something arises in one of two ways: small molecules from the neighbouring material, such as oil, plasticiser or solvent, move into the sealant and soften it there or collect at the bond line, or the surface or components of the neighbouring material block cure and adhesion at the boundary. Either way, the soft zone follows the contact line, which sets it apart from a bead that is under-cured throughout.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: mark the soft and sound areas on a drawing, gather the product names and types of everything the sealant touches along with the application date and weather, and compare them with the compatibility guidance in the sealant's technical data sheet, the TDS.

Hypothesis 1: silicone contact

Consider this hypothesis when another family of sealant, such as polyurethane or a silane-modified polymer, is applied over an old silicone bead that was never removed, or when a two-part platinum-cured silicone is filled against another sealant. A non-silicone sealant is chosen because the joint must be painted, and the silicone left on the substrate ends up covered. Picture a machine cover joint being repaired. A paintable sealant was spread wide over a cracked old silicone bead; a few days later the sealant on the steel is firm, but the strip over the old silicone shifts under the thumb, and lifting it with a knife tip shows a sticky layer underneath.

Silicone refuses other sealants because of its surface. A silicone surface has low surface energy, so liquids placed on it do not spread and wet it well, and even after cure, chains not bound into the network remain and can gather at the surface (Hauer et al., 2024). The new sealant therefore cures without properly wetting the surface at that boundary. The reverse can also happen. Addition-cure silicone, which cures with a platinum catalyst, can have its catalyst blocked and its cure disturbed by tin compounds, sulphur compounds and amines, and the list includes the fatty acid tin salts used in tin-catalysed silicone release coatings (Dow, n.d.). That is why addition-cure silicone poured against a polysulphide sealant, which as its name says carries sulphur, can stay under-cured only at the contact face.

First establish what was under the overlaid area. Cut and lift a little of the soft strip to see whether an old silicone film lies beneath and whether the soft zone matches the width of that film. Lay beads of the same new sealant side by side on a clean substrate and on a piece of old silicone, cure them under the same conditions, measure the hardness of each with a durometer (ASTM International, 2022), and compare adhesion with a hand pull. For addition-cure silicone, the manufacturer also shows how to test, before the main job, whether the materials it will touch block its cure (Dow, n.d.).

Once silicone is shown to be the cause, stop overlaying and strip the old silicone back to the substrate. A thin film can remain even after stripping, so get a cleaning and primer method for that substrate from the new sealant's manufacturer, apply a small section first to check adhesion, then extend to the whole joint. Where the silicone cannot be removed completely, switch to a product the manufacturer states will bond to it. For addition-cure silicone, change the order of work or put another material in between so it does not touch anything that blocks its cure.

Hypothesis 2: bitumen and butyl

Roof flashings, the edges of wall waterproofing and window surrounds are places where sealant often finishes over a bitumen-based self-adhered membrane or bitumen coating, and sealant also meets butyl tape and the butyl primary seal of insulating glass. In insulating glass, polyisobutylene, PIB, a type of butyl rubber, forms the primary seal. Say the edge of a membrane around a roof was pressed down and finished with silicone in midsummer. After a few weeks, only the sealant edge touching the membrane has darkened, and a pull by hand the next year peels it off the membrane starting from that edge.

Bitumen gives off low-molecular-weight oil components that move into the sealant it touches. In a study that placed seven silicones against a bitumen-based self-adhered membrane outdoors, low-molecular-weight compounds from the bitumen moved through the bond line to the sealant surface, oxidised and changed its colour, and the residue collected mainly at the bond line, where it could reduce adhesion (Cronin et al., 2026). In the same study, 8 of 19 specimens had fully released at the bitumen edge after one year, and discoloured specimens showed lower stiffness in dynamic mechanical analysis, though Shore A hardness and tensile tests showed no clear difference. With butyl, migration also runs the other way. An insulating glass industry document screens the effect of components moving from secondary seals and glazing sealants into PIB with a test held at 50°C for 28 days, and after a longer climate-cycling test checks the PIB for softening and adhesion (FGIA & NGA, 2023). The standard for hot-applied pavement joint sealants likewise includes a separate asphalt compatibility test (ASTM International, 2020b).

Start by seeing whether the soft and discoloured areas follow the line of contact with bitumen or butyl. Compare the edge in contact with the middle away from it using the hand-pull method of field adhesion testing (ASTM International, 2020a). The study of bitumen and silicone found that visual and non-destructive checks do not always catch adhesive failure and recommends destructive adhesion tests for each sealant and substrate condition (Cronin et al., 2026). Confirm the product names of the membrane and the butyl product, and ask the sealant manufacturer for compatibility data on that pairing.

If contact with bitumen looks like the cause, separating the two is the basic remedy. The study above advises against placing silicone directly on bitumen-based materials and recommends a separation layer between them, such as a polyethylene-faced membrane or metal flashing (Cronin et al., 2026). Choosing a sealant the manufacturer states can be used with bitumen is another route; an older source describes neoprene sealants as one of the few compatible with asphaltic concrete and bitumen (Persily, 1993). Next to butyl, check with the supplier that the sealant has passed PIB compatibility testing for that pairing.

Hypothesis 3: EPDM plasticiser

In windows, curtain walls and equipment doors, rubber accessories such as EPDM gaskets, setting blocks and spacers touch the sealant. EPDM is a synthetic rubber made from ethylene, propylene and a diene, and is common in gaskets. Look harder if a gasket other than the one on the drawing was fitted because it was to hand. On a run of south-facing windows, white sealant run along the rubber gaskets has turned yellow within a few months only at the edge touching the gasket, and only that edge smears when pressed with a fingertip.

The core of this hypothesis is liquid crossing from the gasket into the sealant. Some sealants, gaskets and other accessories contain fluids or plasticisers that can migrate, and organic plasticiser has been reported migrating from an unapproved EPDM profile into structural silicone. The discolouration in that case came from the ultraviolet light of the test breaking down the migrated plasticiser, and depending on the type and amount of fluid, the sealant's mechanical properties and adhesion can also be affected (Hills & Richards, 2021). The ways rubber compounding ingredients leave the rubber and stain surfaces they touch are measured by a standard set of test methods that separates contact, migration and diffusion (ASTM International, 2025b).

Check the gasket's type and origin first. See from the records whether it is the product on the design or a substitute, and whether the discolouration and soft strip lie only along the gasket contact line. The compatibility test for structural glazing accessories places sealant against the accessory, exposes them to heat and ultraviolet light, and looks at colour change in the sealant, change in adhesion to glass and change in adhesion to the accessory; an accessory that causes discolouration or adhesion loss in the test may do the same in service (ASTM International, 2023a). Ask the gasket supplier whether results from this test exist, and if not, have the test run on the gasket and sealant actually in use.

If the gasket is the cause, resealing alone will not end it. Replace it with a gasket that has passed compatibility testing, and check the setting blocks and spacers as well. For setting blocks, polyethylene, nylon, unplasticised PVC and silicone that contain no fluid or plasticiser are described as suitable (Hills & Richards, 2021). Sorting out with a pull test, before removal, whether only the colour has changed or adhesion has dropped as well makes it easier to set the scope of repair.

Hypothesis 4: old sealant residue

Look at this in repair work where joints are resealed: when old sealant was cut out but a thin film stayed on the joint faces, when a new product was chosen without knowing the old sealant's family, or when oil from an old joint sealant had spread into the substrate. Think of the day the joints in a factory's wall panels are replaced. The crew pulled out the lumps of old sealant, left the glossy film on the joint faces, and put in backer rod and new sealant; a few months later the sealant came away along one face, and the released face stayed sticky.

When old sealant stays, the substrate the new sealant meets is no longer concrete or metal but old sealant. A study of adhesion in resealed joints found that remaining old sealant reduced how far the joint could extend and how well it performed, to a degree that depended on the type, amount and surface energy of the residue (Pagliuca & Hutchinson, 1996). The same study reports that substrate surface energy predicts adhesion, and the surface tension of the uncured new sealant predicts wetting, fairly well. Fluid from old sealant also spreads into the substrate. Tests that placed thirteen commercial sealants on concrete and stone measured migration by the width of the stain the fluid left in the substrate (Snyder et al., 1998).

Look at the released face. If a film of old sealant came away on the back of the new sealant, the new sealant was bonded to that film, not to the substrate. Find the old sealant's family in the construction records, and if there are none, send a piece to a laboratory to identify it by infrared spectroscopy. The study of bitumen and silicone above analysed the bond line with the same method (Cronin et al., 2026). Before filling the joints at large, apply one or two sections first, let them cure and confirm adhesion with a field adhesion test (ASTM International, 2020a).

The first remedy for residue is to remove it mechanically down to bare substrate. Grind off the film left after cutting with a grinder or wire brush, and wipe away dust and grease by the method the sealant manufacturer specifies. If the old sealant was silicone, the remaining film brings the silicone problem above with it, so remove it all the more carefully. Where oil has soaked deep into a porous substrate, cut that part out or agree a primer for it with the manufacturer.

Hypothesis 5: rod or solvent misuse

The subjects here are the backer rod, the cylindrical foam placed at the bottom of a joint to set sealant depth, and the solvent and primer used to clean the joint before sealing. Look at it where whatever foam was to hand served as backer rod, where the rod's skin was torn as it was pushed in, or where sealant went in before the cleaning solvent or primer had dried. Take a day when, to keep to schedule, closed-cell backer rod was jabbed into the joints with the tip of a screwdriver and the sealant went in straight away. A few days later the surface has cured, but the deep part feels spongy under pressure, and a cut shows small bubbles gathered just above the backer rod.

Backer rod limits sealant depth, gives a firm base to tool the sealant against, and stops the sealant bonding to the bottom of the joint. To do that it must not absorb water, must not give off gas that forms bubbles in the sealant, and must be compatible with the sealant. If closed-cell rod is torn during installation, gas from the ruptured cells can be pumped into the uncured sealant as temperature changes, and the bubbles can reduce the sealant's cohesion (Persily, 1993). A pavement joint repair manual also states that backer rod must be non-reactive and non-absorptive, and that rod reacting with some sealants can cause bubbles or staining (Evans et al., 1999). The backer rod specification divides rod into closed-cell, open-cell and bicellular types but does not address compatibility with the sealant, so that judgement has to be made separately (ASTM International, 2023b).

Solvent and primer cause trouble at the same boundary. Most sealant adhesion problems come from a substrate that is dirty or wet when the sealant goes on, with dirty or wrong solvent and contaminated rags named among the causes. Too much primer, the wrong primer, or sealing before the primer has dried also leads to adhesion problems (Persily, 1993). Where bubbles gather by the backer rod, look at the rod first; where the adhesion problem lies along the joint faces, look at solvent and primer first.

Cut across the joint and examine the section. See where the soft layer and bubbles have gathered, whether the backer rod's skin is torn or wet, and what cell structure the rod has. The rod's potential to give off gas can be measured separately by a standard test method (ASTM International, 2019). From the work log, find the cleaning solvent used, the time the primer went on and the time the sealant went in, and compare them with the drying time in the primer's TDS.

When the rod has to change, choose the type the sealant manufacturer recommends, and do not puncture it with sharp tools or stretch it until it tears during installation. Keep joints with open-cell rod from getting wet with rain or cleaning water, and dry or replace the rod if it does. If solvent and primer are the cause, clean with the solvent the sealant manufacturer specifies and clean rags, and fill only after the primer has had its full drying time from the TDS.

Finding the cause

Five hypotheses do not need five investigations at once. Rule them out one at a time, starting with what is easy to see. What the soft area touches can be told at once by eye and fingertip, and the product names of the materials in contact and the work log are on paper. Cutting sections or sending samples to a laboratory comes after that.

The first clue is the shape of the soft zone. A soft strip matching the width of overlaid old silicone, or limited to the face where silicone was poured against another sealant, points to silicone contact; one that follows the edge against a bitumen membrane or butyl tape points to oil from that material; and one along the gasket line that has also changed colour points to plasticiser from the gasket. An old film coming away on the released face points to old sealant left behind, and softness only in the deep part with bubbles above the backer rod points to the rod. If the whole bead is soft regardless of contact, look first at conditions that slow cure itself, such as mixing, temperature and humidity, rather than at these five.

If the shape does not settle it, run a control test. Lay small beads of the same sealant on clean glass or metal and on each suspect material, cure them at the same temperature and humidity, and compare durometer hardness and hand-pull adhesion side by side (ASTM International, 2022). Migration takes time, so do not judge after a day or two. Accessory compatibility tests speed the process up with heat and ultraviolet light, and the insulating glass industry's PIB test runs for 28 days at 50°C (FGIA & NGA, 2023).

After the cause is corrected and the joint resealed, run a field adhesion test on a section under the same conditions as the first soft area, and look at the same place again a few weeks later (ASTM International, 2020a). As discolouration appeared after about six weeks in the bitumen study, changes from migration may not show right after application (Cronin et al., 2026).

The hypotheses can overlap. If the old sealant was silicone, its remaining film brings the same problem as sealant over silicone, and when a bitumen membrane and an EPDM gasket share one joint, it is hard to tell whose oil it is. Components can spread even between materials that do not touch (FGIA & NGA, 2023), so remove or change one material at a time and measure hardness and adhesion on the same basis each time. When causes seem to overlap, clear away what can be cleared, such as old film and leftover solvent, first, and the remaining hypotheses become easier to separate.

Limits and cautions

Compatibility varies by formulation, not by family. Even among silicones, results against bitumen differed by product, and five of the eight first-year adhesive failures came from one manufacturer's products (Cronin et al., 2026). Whether a pairing works is therefore settled by the manufacturer's confirmation or a test on the actual sealant and neighbouring products, and the guide on using joint sealants also says to consult the manufacturer about applications (ASTM International, 2025a). Where sealant carries load, as in structural glazing, do not close out a repair on site judgement alone; have the designer and manufacturer review it.

Check the flammability and vapour hazards of cleaning solvents and primers in each product's safety data sheet, the SDS, and follow it for ventilation, control of ignition sources, protective gloves and eye protection. Grinding out old sealant raises dust, so wear a dust mask, and have materials of unknown composition, such as joint sealants in old buildings, analysed before grinding. Work on high joints only with fall protection in place.

Sources

  1. ASTM International. (2019). ASTM C1253-14(2019), Standard test method for determining the outgassing potential of sealant backing. https://store.astm.org/c1253-14r19.html
  2. ASTM International. (2020a). ASTM C1521-19(2020), Standard practice for evaluating adhesion of installed weatherproofing sealant joints. https://store.astm.org/c1521-19r20.html
  3. ASTM International. (2020b). ASTM D5329-20, Standard test methods for sealants and fillers, hot-applied, for joints and cracks in asphalt pavements and portland cement concrete pavements. https://store.astm.org/d5329-20.html
  4. ASTM International. (2022). ASTM C661-15(2022), Standard test method for indentation hardness of elastomeric-type sealants by means of a durometer. https://store.astm.org/c0661-15r22.html
  5. ASTM International. (2023a). ASTM C1087-23, Standard test method for determining compatibility of liquid-applied sealants with accessories used in structural glazing systems. https://store.astm.org/c1087-23.html
  6. ASTM International. (2023b). ASTM C1330-23, Standard specification for cylindrical sealant backing for use with cold liquid-applied sealants. https://store.astm.org/c1330-23.html
  7. ASTM International. (2025a). ASTM C1193-25, Standard guide for use of joint sealants. https://store.astm.org/c1193-25.html
  8. ASTM International. (2025b). ASTM D925-14(2025), Standard test methods for rubber property—Staining of surfaces (contact, migration, and diffusion). https://store.astm.org/d0925-14r25.html
  9. Cronin, K., Horton, E., Schofield, M., & Kim, S. (2026). When sealants meet waterproofing: A sticky situation. IIBEC Interface. https://iibec.org/publication-post/when-sealants-meet-waterproofing-a-sticky-situation/
  10. Dow. (n.d.). FAQ: Platinum catalyzed silicone inhibitors. Retrieved November 2026. https://www.dow.com/en-us/faq/platinum-catalyzed-silicone-inhibitors.html
  11. Evans, L. D., Smith, K. L., & Romine, A. R. (1999). Materials and procedures for repair of joint seals in portland cement concrete pavements: Manual of practice (FHWA-RD-99-146). Federal Highway Administration. https://rosap.ntl.bts.gov/view/dot/40384
  12. Fenestration and Glazing Industry Alliance [FGIA] & National Glass Association [NGA]. (2023). Compatibility testing of insulating glass PIB primary sealant with respect to glazing materials (IGMA TB-1300-23 / NGA FB75-23). https://www.glass.org/sites/default/files/2023-06/NGA-FB75-23_IGMA-TB-1300-23_Compatibility_Testing_PIB_final.pdf
  13. Hauer, L., Naga, A., Badr, R. G. M., Pham, J. T., Wong, W. S. Y., & Vollmer, D. (2024). Wetting on silicone surfaces. Soft Matter, 20(27), 5273–5295. https://doi.org/10.1039/d4sm00346b
  14. Hills, A., & Richards, J. (2021). Why structural silicone sealants play a crucial role in structural glazing. Sika UK. Retrieved November 2026. https://gbr.sika.com/en/media/blogs/structural-silicone-sealants.html
  15. Pagliuca, A., & Hutchinson, A. (1996). Adhesion properties of sealants in resealed joints. ASTM International symposium paper, pp. 109–128. https://doi.org/10.1520/STP16298S
  16. Persily, A. K. (1993). Envelope design guidelines for federal office buildings: Thermal integrity and airtightness (NISTIR 4821). National Institute of Standards and Technology. https://nvlpubs.nist.gov/nistpubs/Legacy/IR/nistir4821.pdf
  17. Snyder, R., Badour, R., Carbary, L. D., & Wolf, A. T. (1998). Comparison of various test methods for assessing the long term fluid migration potential for sealants. ASTM International symposium paper, pp. 210–218. https://doi.org/10.1520/STP15679S

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.