KALTECKOREA

BlogApplication notes

Why does floor joint sealant get torn out by forklift traffic?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Sealants & Damping

Refilling with the same sealant and moving on is the easy response to joints torn out by forklifts, but if the condition that let them tear stays, the refilled joints tend to tear again in the same traffic lanes. What actually lies behind it can be joint material too soft to support the wheels, spalled joint edges, chemicals and oil, the wrong fill depth or level, or traffic let on before cure, and sometimes two or more at once.

Background

Every joint across a warehouse aisle thumps as a forklift crosses it. The material that filled the joints has been torn out in places, leaving empty grooves, and the concrete at their edges breaks away so the grooves keep widening. Each time a wheel drops into one, the load and the truck jolt, and dust and debris collect in the empty groove. Joint material that has come away from the joint walls looks poor and can create hygiene problems (Van der Merwe, 2012), and refilling means closing that aisle to work on it.

Joints in a concrete floor are grooves sawn or formed so that the slab cracks at chosen places as it dries and shrinks. The semirigid epoxy or polyurea filler placed in them protects the joint edges from spalling under the wheels of forklifts, pallet trucks and carts and carries load across the joint, and to do that it has to be relatively stiff compared with a joint sealant (CPC, 2020). Slabs keep shrinking for years, most of it within the first 4 years and the largest part in the first year, especially the first 90 days, so the floor construction guide advises deferring joint filling as long as possible (ACI, 2015).

Joint material therefore sits between two forces: hard wheels striking the edges from above, and the slab shrinking and slowly opening the joint from the side. It is torn out in two ways as well: either the material itself cannot withstand the wheels, or the edges and walls that held it fail first.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: walk the aisles and mark damaged joints on a drawing, gather the joint material's product name, the date it went in, the age of the slab at filling and the time traffic was let on, and compare them with the material's technical data sheet, the TDS.

Hypothesis 1: material too soft

The subject here is a floor where a soft elastomeric sealant, the kind used in exterior wall or partition joints, went into floor joints crossed by forklifts: a sealant chosen because it follows movement well, placed under the wheels. Think of a new warehouse where the elastomeric sealant left over from the wall joints was used to fill the floor joints too. A few months later the sealant in joints crossing the forklift lanes has been pressed and shredded by the wheels, while joints in the walkways used only by people are intact.

The building sealant specification classifies sealants for joints that carry pedestrian and vehicle traffic separately, and states that such joints call for attention to material selection, joint design, manufacturer involvement and field testing together (ASTM International, 2024). In a floor joint under wheels, a soft material cannot support the edges and is pushed aside, so the hard wheel strikes the concrete edge directly. Semirigid filler is made stiff to protect that edge, but in exchange it can barely stretch sideways and its adhesion is kept low so that it does not weld the two slabs together. When the joint opens a long way, the filler is therefore bound to come away from the wall or tear internally (CPC, 2020).

Compare joints in the lanes with the rest. See whether tearing concentrates where forklift wheels run, and measure the remaining material with a durometer against the hardness in the TDS. The durometer test is an empirical test meant mainly for quality control, so the comparison only holds when sound and torn joints are measured the same way side by side (ASTM International, 2021a). The sealant hardness test also states that its value is not a measure of wear resistance, so treat hardness as a starting point for judgement only (ASTM International, 2022a).

If soft sealant is the cause, consider changing joints under forklift traffic to semirigid epoxy or polyurea filler. Strip the old sealant back to the substrate, and follow the hardness and installation conditions in the filler manufacturer's TDS. If filling happens while the slab is still shrinking substantially, treat separation from the wall as expected, and settle in the contract documents beforehand when joints will be refilled and who carries the repair and its cost (CPC, 2020).

Hypothesis 2: spalled joint edges

Joint edges break by several routes, from the ground under the floor to the quality of the work. Look at floors with weakly compacted subgrade, construction joints whose edges were damaged when formwork was stripped, joints where an uneven floor level makes wheels hit a step, and junctions where loaded forklifts often turn. Say one joint in front of a loading area tears out far more often than the rest. Up close, both edges have broken away, leaving the joint material at the bottom of a dished groove below floor level, and the forklift wheels drop into that groove and climb out again at every pass.

Once an edge breaks, the joint material loses the wall it was bonded to, and the wheel strikes the lip of the broken groove. A study of joint damage in warehouse floors found that as forklift wheels cross a joint, wheel load and impact energy pass into the joint edge, and grouped the causes in three. Subgrade that is poorly compacted, or loses fines washed out by water, lets the slab deflect more; uneven trowelling leaves the floor level irregular; and joints where formwork was stripped badly start life with damaged edges (Van der Merwe, 2012). The same study also took up joint material coming away from the joint walls.

Start with the edges. Walk the joints, log the length and depth of each broken edge, and see whether the broken places coincide with where the material has torn out. The pavement joint manual says to measure joint width, depth and material thickness during inspection, and that full-depth spalls can be found by gently inserting a dull knife into the spall and seeing whether the tip passes below the sealant (Evans et al., 1999). Lay a straightedge across the slabs on both sides to check for a step, and watch whether the two sides move separately as a loaded forklift crosses.

Refill only the joint material and leave the broken edges, and the wheels keep striking the same lip. Rebuild the edges first with a repair resin mortar so the joint walls are straight, then fill, and make sure the repair faces are clean, free of dust and moisture, or the filler will not bond. Most sealant adhesion problems have been traced to a substrate that was dirty or wet when the sealant went on (Persily, 1993). If the step or deflection is large, it is not something joint material can fix, so review load transfer and subgrade condition with a concrete floor specialist.

Hypothesis 3: chemicals and oil

Joints where forklifts leaking hydraulic oil park, in battery charging areas, along aisles where floor scrubbers spray detergent, and on routes that carry process chemicals need looking at separately. If only those joints fail first on an otherwise uniform floor, this hypothesis moves to the front. The joint in front of a charging area is a typical sight. Only there has the joint material gone tacky and swollen, with deep wheel ruts in it; hydraulic oil stains spread across the parking bay next to it, and the material has been torn out by the wheels starting from the joints the stain reached.

Rubber-like materials in contact with a liquid can absorb it or have their own components dissolve out, and their properties can deteriorate. That is why the standard test comparing how rubber withstands liquids separately measures the change in mass, volume, tensile strength, elongation and hardness after immersion, and the amount extracted by the liquid (ASTM International, 2021b). Concrete pavements where fuel may be spilled have their own specification for fuel-resistant joint sealants, which tests bond while immersed in fuel (ASTM International, 2021c), and the European specification for cold-applied joint sealants likewise separates normal and fuel-resistant types while leaving uses such as petrol stations and the chemical industry outside its scope (BSI, 2005). In other words, joint material for ordinary floors cannot be assumed to withstand every chemical and oil.

See whether the damage concentrates where chemicals or oil reach. Check whether the damaged material has swollen, gone tacky or, the other way round, turned hard and crumbly, and compare its hardness with sound joints. Establish what reaches it by collecting the list of chemicals and oils used at charging areas, cleaning equipment and process plant, with their safety data sheets, the SDS, and compare them with the joint material manufacturer's chemical resistance data. For chemicals not in the data, have specimens of the material immersed in them. The chemical resistance test for resin-based materials looks at specimen mass and appearance, change in the test liquid and compressive strength after immersion, and says the results should guide, but not be the sole basis for, material selection (ASTM International, 2020).

With chemicals and oil, stopping the leaks comes first. Repair equipment leaking hydraulic oil, and set a procedure for wiping up spills at once in charging and cleaning areas. Change the joints in those zones to a material the manufacturer states will withstand the chemicals involved, and use a different grade of material from the general floor where fuel or aggressive chemicals reach. Before refilling, grind oil-soaked joint walls back to clean concrete.

Hypothesis 4: wrong depth or level

How deep the joint material was placed, and at what level, also needs checking: when the lower part of the joint was packed with sand or backer rod under schedule pressure and only a thin layer went on top, when sealant was placed thick or smeared over the floor, or when the top was left above or below floor level. Take a section where, with repairs on a tight schedule, the lower part of the joints was filled with sand and only the top covered with filler. One season later the filler in that section has lifted out whole like a thin strip, exposing the sand beneath.

Because a semirigid filler's job is not to stretch but to support the edges against wheel impact (CPC, 2020), it can hardly do that job if the filler does not back the edge the wheel presses on. For elastomeric sealant, the ratio of width to thickness, the shape factor, matters. The pavement joint manual says a thick band cannot stretch as far as a thin one before tearing, so the shape factor should follow the manufacturer's recommendation; it also states that sealant smeared over the surface is worn away by traffic within 1 to 3 years, after which tyres pull the sealant from the joint edge and lead to adhesion failure. The same manual says silicone sealant should never be overbanded or left flush, and reports the manufacturers' recommendation of a recess of at least 7 to 10 mm below the surface to avoid early adhesion failure (Evans et al., 1999).

Cut out the joint material at one spot and measure the depth. See how deep the saw cut is, how deep the material goes and what lies beneath it, and check with a straightedge whether the top is level with the floor. If strips have lifted out, compare their thickness with the minimum depth in the TDS. Finding in the installation records the sections filled the same way on the same day shows whether the damage clusters there.

Refill to the depth, and with the support method, that the joint material manufacturer sets. Fill semirigid filler to the specified depth, and once cured, shave the top flush with the floor so wheels do not catch on a lip. For joints using elastomeric sealant, match shape factor and thickness to the manufacturer's recommendation, and set the level so that wheels do not grind the top directly.

Hypothesis 5: traffic before cure

This becomes a problem with the morning shift that follows a night repair, in cold stores and freezers where cure takes longer, and on sites that cannot keep an aisle closed for long. The joints were refilled overnight, and the closed aisle was reopened when the morning shift began. By afternoon, wheel marks are printed in the top of the joint material in the lanes, and in places the uncured interior has been squeezed out and smeared across the floor by the wheels.

There is a gap between when joint material dries on the surface and when it has cured through. A separate standard test measures the time until the sealant surface no longer comes away on the hand, the tack-free time (ASTM International, 2022b). According to the pavement joint manual, non-self-levelling silicone sealant is generally tack-free within 90 minutes above 4°C and cures within 7 days, and the manual advises opening to traffic only once the surface is tack-free or skinned, waiting longer where large deflections are expected (Evans et al., 1999). Movement during cure is a problem too. A study that cycled a silicone sealant during cure concluded that how far cure had progressed when movement began appeared to be the key variable for performance (White et al., 2010).

From the records, find when the joints were filled, when traffic was let on and the floor temperature in between, and compare with the time to traffic in the TDS. See whether damage is confined to sections refilled that day, and whether wheel marks or squeeze marks are printed in the top surface. Leave a sample filled the same day from the same batch somewhere without traffic and measure its hardness at intervals to estimate how far cure had gone when traffic was let on (ASTM International, 2022a).

Where traffic before cure seems to be the cause, keep the refilled joints closed until the time to traffic in the TDS has passed. In cold warehouses the same product takes longer, so set the time by floor temperature rather than air temperature, and ask the manufacturer whether a product for low temperatures exists. If an aisle cannot stay closed for long, fill alternate sections in turn, or choose a fast-curing product and keep to its time to traffic.

Finding the cause

There is no need to investigate all five hypotheses at once. Rule them out starting with what is easy to measure. The damage map, the material's product name, the installation records and the time traffic was let on can be gathered at once, and hardness and depth can be measured on a single piece of joint material. Investigations that need equipment and specialists, such as subgrade and slab deflection, come after.

The location and shape of the damage are the first clues. Shredding only in joints across forklift lanes points to soft joint material; broken edges coinciding with torn-out material point to spalled edges; and swelling or tackiness around charging areas or oil stains points to chemicals and oil. A thin strip lifted out whole, or a top left above or below the floor, points to fill depth or level, and wheel marks only in sections refilled on a given day point to traffic before cure. If the filler has come cleanly off a joint wall or split down the middle, it may be the result of the slab shrinking and opening the joint, separate from all five hypotheses (CPC, 2020).

If that still does not settle it, set up trial sections that change only one condition. Fill a few joints in the same aisle with a different material, fill the same material deeper, or let traffic on later, and after a set period measure the length of damaged joint on the same basis. Change several conditions at once and there is no telling which one worked.

After the repair, pick the lane joints to follow and walk them at set intervals, recording broken edges, gaps at the walls and wheel marks. The job is done only when as much time has passed as it took the first damage to appear, with no new damage in the same places. For joints filled early, handle separation caused by slab shrinkage in the meantime separately, as part of the maintenance schedule.

The hypotheses can overlap. When wheels strike the edge directly through soft material, the edge breaks, and a broken edge in turn makes the material easier to tear out. Material softened by oil looks much like material that was too soft from the start, and shallow filler is more easily damaged by traffic before cure. In such cases, correct the geometry of the joint first, its edges and depth, and then settle the material and the time to traffic, because in a joint of the wrong shape no material can perform as it should.

Limits and cautions

Hardness, fill depth, time to traffic and chemical resistance differ by product, so numeric decisions follow that product's TDS. Figures from the pavement joint manual come from road pavements carrying rubber tyres, so do not carry them over unchanged to plant floors carrying hard wheels. Slab deflection, subgrade settlement and widely broken joints can be structural problems, so leave them to a concrete floor specialist, and since slabs shrink over several years (ACI, 2015), plan separation in early-filled joints as a maintenance item rather than a defect.

Handle epoxy and polyurea joint materials and cleaning solvents with gloves, eye protection and ventilation as set out in each product's SDS. Grinding out old material and edges raises concrete dust, so use dust extraction and dust masks. Put signs and barriers around the work area to stop forklift traffic, and keep equipment out of the lane while anyone is working in it.

Sources

  1. American Concrete Institute [ACI]. (2015). Guide to concrete floor and slab construction (ACI 302.1R-15). American Concrete Institute.
  2. ASTM International. (2020). ASTM C267-20, Standard test methods for chemical resistance of mortars, grouts, and monolithic surfacings and polymer concretes. https://store.astm.org/c0267-20.html
  3. ASTM International. (2021a). ASTM D2240-15(2021), Standard test method for rubber property—Durometer hardness. https://store.astm.org/d2240-15r21.html
  4. ASTM International. (2021b). ASTM D471-16a(2021), Standard test method for rubber property—Effect of liquids. https://store.astm.org/d0471-16ar21.html
  5. ASTM International. (2021c). ASTM D7116-16(2021), Standard specification for joint sealants, hot applied, jet fuel resistant types, for portland cement concrete pavements. https://store.astm.org/d7116-16r21.html
  6. ASTM International. (2022a). ASTM C661-15(2022), Standard test method for indentation hardness of elastomeric-type sealants by means of a durometer. https://store.astm.org/c0661-15r22.html
  7. ASTM International. (2022b). ASTM C679-15(2022), Standard test method for tack-free time of elastomeric sealants. https://store.astm.org/c0679-15r22.html
  8. ASTM International. (2024). ASTM C920-18(2024), Standard specification for elastomeric joint sealants. https://store.astm.org/standards/c920
  9. British Standards Institution [BSI]. (2005). BS EN 14188-2:2004, Joint fillers and sealants — Specifications for cold applied sealants. https://knowledge.bsigroup.com/products/joint-fillers-and-sealants-specifications-for-cold-applied-sealants
  10. Concrete Polishing Council [CPC]. (2020). Separation of semirigid concrete floor joint fillers (CPC Position Statement #4). American Society of Concrete Contractors; published in Concrete International. https://ascconline.org/Portals/ASCC/CPC-PS-4-Semirigid-Floor-Joint-Fillers.pdf
  11. Evans, L. D., Smith, K. L., & Romine, A. R. (1999). Materials and procedures for repair of joint seals in portland cement concrete pavements: Manual of practice (FHWA-RD-99-146). Federal Highway Administration. https://rosap.ntl.bts.gov/view/dot/40384
  12. Persily, A. K. (1993). Envelope design guidelines for federal office buildings: Thermal integrity and airtightness (NISTIR 4821). National Institute of Standards and Technology. https://nvlpubs.nist.gov/nistpubs/Legacy/IR/nistir4821.pdf
  13. Van der Merwe, E. M. (2012). Behaviour of floor joint edges under hard-wheeled loads [Master's dissertation, University of Johannesburg]. https://ujcontent.uj.ac.za/esploro/outputs/graduate/Behaviour-of-floor-joint-edges-under/9910214107691
  14. White, C. C., Hunston, D. L., & Williams, R. S. (2010). Studies on the effect of movement during the cure on the mechanical properties of a silicone building joint sealant. Polymer Engineering & Science, 50(1), 113–119. https://doi.org/10.1002/pen.21518

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.