KALTECKOREA

BlogApplication notes

Why does sealant in continuously wet joints soften and let go?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Sealants & Damping

Refilling the joint with the same sealant is the usual response when sealant under water softens or lets go, but if the conditions by which water weakened the sealant or its bond remain, the new sealant goes the same way. What actually lies behind it can be hydrolysis of the polymer by water, water reaching the interface, a primer not made for immersion or badly applied, chlorine and disinfectants, or warm water, and sometimes two or more at once.

Background

A routine inspection drains a tank or pool, and the movement joint sealant in the floor and walls has softened so much that a finger sinks into it. In places it has come away from one side, leaving a gap between sealant and concrete. Water leaking through that gap wets the concrete, reinforcement and waterproofing behind the joint, and repair means draining, drying the substrate, waiting for the new sealant to cure and refilling. For a pool, a water treatment works or a wastewater plant, the facility stands idle meanwhile.

A permanently submerged joint lives under different conditions from a façade joint that is wetted by rain and dries out. Water diffuses into the sealant, where it can react with the polymer or swell it, and passes through to reach the interface with the substrate. The standard continuous immersion test keeps sealant in hot liquid to assess its durability and its adhesion to the substrate. It does not include the effect of hydrostatic pressure or joint movement, and because adhesion lost while wet can return while dry, results may differ from joints that cycle between wet and dry (ASTM International, 2020).

That is why sealants for structures permanently under water, such as potable water reservoirs, face stricter demands for hydrolytic stability, resistance to flow under load, retention of elasticity and adhesion (Randazzo, 1992). Softening means the body of the sealant has weakened; letting go means the interface has. Separating the two narrows the cause sharply.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: check whether the technical data sheets, the TDS, for the sealant and primer used state continuous immersion as a use, and compare them with the facility's records of water temperature, disinfection method and pH.

Hypothesis 1: polymer hydrolysis

This hypothesis comes to mind first when a general-purpose façade sealant was used as it is in a tank or channel, especially a polyurethane made with polyester raw materials. It typically shows as sealant that was sound after installation and softens slowly as it stays under water. Drain a channel at a wastewater plant and cut into a wall movement joint. The surface is tacky, and the section is evenly soft from the face well into the depth, smearing onto the blade. The same sealant higher up the channel wall, out of the water, is still elastic.

Hydrolysis is a reaction in which water molecules break bonds in the polymer chain. As the chains are cut shorter, the sealant loses elasticity and strength and turns soft and tacky. A review of polyurethane elastomer degradation treats hydrolysis as one of the main degradation routes and shows that stability depends strongly on building blocks such as the soft-segment raw material, whether polyester, polyether or polycarbonate. The polyester types, with their ester bonds, are especially prone to hydrolysis (Xie et al., 2019). Other families vary with formulation as well. A study of polysulfide sealants in water-retaining structures found that polymer content, curative type and other ingredients govern long-term performance in water (Lee et al., 1992).

First establish whether the whole body of the sealant has softened. Cut the joint, measure hardness at the face, middle and bottom of the section with a Shore A durometer, and compare with the same sealant where it is not submerged. If it is evenly soft through the depth while sealant out of the water is sound, water has changed the sealant itself. Confirm the product family, the uses listed in the TDS, and whether continuous immersion test data exist.

If hydrolysis is confirmed, refilling with the same product only buys time. Choose with the supplier a sealant tested for continuous immersion, and get data on the liquid, temperature and duration of that test. Remove the softened sealant completely so none is left on the substrate, then reinstall.

Hypothesis 2: water at the interface

When the body of the sealant is still elastic but has come cleanly off the substrate, turn attention to the interface. It shows up readily on substrates that hold water, such as concrete, in joints installed before the substrate had dried, and in joints where water pressure acts to push the sealant off the substrate. Lift the sealant in a water tank wall joint with a knife point and it looks like this: the sealant stretches like rubber yet peels off the concrete face in a clean strip, and the exposed concrete is wet and slick.

Water reaches the interface either through the sealant or from the substrate side, and the interface itself is an easy path. In an experiment comparing bulk specimens and joints made with the same epoxy adhesive, the joints took up water faster, which was explained by surface tension near the metal oxide and polymer interface adding to the driving force for water entry (Zanni-Deffarges & Shanahan, 1995). Water gathered at the interface can push the adhesive off the substrate. A study of water-induced failure in steel joints bonded with epoxy used thermodynamic calculation to predict when the interface becomes unstable under water (Gledhill & Kinloch, 1974). In joints with water pressure acting from behind the substrate, the push on the interface may be greater still.

Looking at the separated face is the starting point. If no sealant at all remains on the substrate, it is an interfacial failure; check then whether the substrate face is wet and whether water seeps out from behind the joint. On runs that are still bonded, cut a short tab of sealant free and pull it by hand, comparing run by run how and at what point it lets go. Find the records of substrate moisture and cleaning at installation as well.

For an interface problem, prepare the substrate again from the start. Grind off laitance and contamination, install only once the substrate has dried to the condition the supplier specifies, and where water comes from behind the substrate, close that path first. Before refilling, make a test piece on the same substrate, keep it under water for a while and pull it, which shows in advance whether the interface holds.

Hypothesis 3: primer at fault

Look into this hypothesis when a primer from façade work went straight into tank joints, when primer was skipped, or when it was applied too thick or sealant went on before it had dried. A good example is pool repair work where a different primer left on site was used on some runs only. A season after refilling, sealant has lifted along the joint edges on those runs alone, while the rest is unchanged.

Primer is a thin layer that links substrate and sealant, and many primers use silane coupling agents. The bonds a silane forms with inorganic surfaces such as glass or concrete can hydrolyse in water and re-form once the water leaves; they are reversible (Plueddemann, 1991). In joints that cycle between wet and dry there is a chance for them to re-form, but in a joint that is always submerged that chance rarely comes. The continuous immersion standard likewise notes that for some sealant and substrate pairs, adhesion lost while wet is regained while dry (ASTM International, 2020). Work on sealants for water-retaining structures likewise treats the role of the primer as its own factor in keeping adhesion over time (Lee et al., 1992).

From the installation records, find the name and lot of the primer used, the amount applied and the drying time, and check whether its TDS lists continuous immersion. If the lifted runs and the sound runs used different primers, that alone is a strong clue. Look also at whether the primer stayed on the substrate or came away on the sealant. Primer left on the substrate means the weak link was between primer and sealant; primer on the sealant means it was between primer and substrate.

When the primer turns out to be the weak point, change to the one the sealant supplier specifies for continuous immersion with that sealant and substrate. Keep to the application rate and drying time, and place the sealant within the primer's open time. When work is split into phases, standardise on one primer so no other product gets mixed in on site.

Hypothesis 4: disinfectant attack

Pool water is managed by filtration together with chlorine or other disinfectants (WHO, 2006). This hypothesis concerns facilities where the water carries an oxidant, such as swimming pools, chlorine contact tanks at water treatment works and cooling water systems dosed with disinfectant. It is more likely where shock treatment, a large one-off dose of chlorine, is frequent, or where joints sit near the dosing point. Say an outdoor pool is drained at the end of a season that saw several shock treatments. The sealant surface comes off like chalk, white and powdery, and below it the sealant is tacky. Joints at the shallow end, which had long sun exposure, are worse than those at the deep end.

Disinfectants are oxidants, so they attack not only microbes but polymer chains and the additives within them. In a study of polyethylene pipes carrying drinking water disinfected with chlorine dioxide, the disinfectant consumed antioxidant at the inner wall and oxidised the polymer (Colin et al., 2009). A US Navy report on failed polysulfide sealant in pool joints concluded that chlorine, sunlight and shock treatment together contributed to the breakdown, that high chlorine during shock treatment produces severe chalking, and from bleach immersion tests that urethane should outperform polysulfide (NFESC, n.d.). Even a pool silicone sold as chlorine-resistant depends, its supplier states, on the water's pH and free chlorine for that resistance (Sika, n.d.).

The facility's disinfection log is the first evidence. Look at the disinfectant type, daily free chlorine and pH readings, and the number and strength of shock treatments, and compare them with the conditions in the sealant TDS or given by the supplier. Examine the sealant face and section separately. If a white powder or tacky layer sits only at the face while the interior is elastic, the weight shifts from water itself towards disinfectant and sunlight. Compare runs by distance from the dosing point and by sun exposure to see whether condition varies with them.

Once disinfectant is pinned down, address water management and product choice together. Keep free chlorine and pH within set ranges, shock-treat only as often as needed, and site dosing points away from joints. When reinstalling, give the supplier the facility's actual disinfection method, concentrations and shock-treatment practice, and choose a product tested under those conditions.

Hypothesis 5: warm water

This covers warm pools and spas, hot spring baths, channels carrying process-heated water, and shallow tanks warmed by summer sun. It can show up within one facility as a difference between the warm and cold sides. Picture a bathhouse where the cold and hot plunge pools were sealed on the same day with the same sealant. Some years on, the hot pool joints have softened and let go in places, while the cold pool joints are still elastic.

As temperature rises, both the rate at which water enters the sealant and the interface and the rate at which it cuts chains increase. The standard continuous immersion test uses hot liquid precisely to accelerate degradation with heat, which is why it predicts long-term durability only when the actual service temperature is well below the test temperature (ASTM International, 2020). Put the other way round, if the real water temperature is close to or above the test temperature, the test result does not guarantee service life. The polyurethane degradation review likewise treats hydrolysis as degradation that speeds up with temperature and humidity (Xie et al., 2019). That is why hydrolysis, water at the interface and primer weaknesses all show up earlier in warm water.

Pull the water temperature records to find normal and peak temperatures, and compare them with the service temperature range in the TDS and the temperature of the supplier's immersion tests. If the same sealant was used in both cold and warm water, set the hardness and adhesion of the two side by side. If only the warm side has failed, this hypothesis is strong, and whether the failure is softening or letting go reveals which other cause acted with it.

The core of the remedy is a product with test evidence at that temperature. Tell the supplier the actual peak water temperature and ask for immersion test data at or above it. Where the temperature can be lowered, as with process water, lowering the temperature of water reaching the joint also extends life, and joints on the warm side get a shorter inspection interval.

Finding the cause

There is no need to investigate all five hypotheses at once. Rule out first what paperwork can confirm. Whether the sealant and primer TDS list continuous immersion, and whether water temperature and disinfection records fall within those conditions, can be checked before the facility is drained. Cutting joints to examine sections and pull tests come after draining.

The first fork comes once the sealant is in hand. Evenly soft through the section points to a change in the body of the sealant, such as hydrolysis; elastic but parted from the substrate points to water at the interface and the primer. A white powder or tacky layer only at the face, with a sound interior, points to disinfectant and sunlight. Where the primer stayed on the separated face narrows the interface causes further.

Next is where the damage lies. Clustering in warm water points to temperature; clustering near dosing points or at the sunlit shallow end points to disinfectant; clustering in a particular phase of work points to the primer and substrate preparation on that phase. Sound sealant of the same kind where it is not submerged serves as a reference showing the cause lies in the water and what it carries.

If that still does not settle it, run control trials on test pieces. Make candidate sealant and primer combinations on the same substrate and immerse them separately in the facility's actual water and in tap water, at the actual temperature and in cold water, measuring hardness and pulling them at set intervals. Change only one condition at a time, or there is no telling which one made the difference. The final check is to measure the reinstalled joints the same way at the first routine inspection.

The hypotheses can overlap. Warm water speeds up both hydrolysis and water at the interface, and sealant whose face has been damaged by disinfectant lets water in more easily. In such cases put the sealant and primer right first, with a combination tested for continuous immersion at the actual temperature and disinfection conditions, then refine substrate preparation and water management on that basis. While the product does not suit the conditions, the effect of other measures is buried in fast degradation and cannot be compared.

Limits and cautions

Resistance to continuous immersion, allowable water temperature, disinfectant concentration and pH range, and primer type and drying time differ by product, so numeric decisions follow the TDS for the sealant and primer and the supplier's recommendations. Laboratory immersion tests leave out hydrostatic pressure and joint movement, so their results do not translate directly into service life. For tanks holding drinking water, confirm that the sealant and primer meet that country's requirements for contact with potable water, and where leakage has spread to reinforcement corrosion or the ground, get a structural engineer's assessment.

Safety matters too. A drained tank or channel may be a confined space, so test for oxygen and harmful gases, ventilate and post a standby person before entry. Mixing chlorine disinfectants with acidic cleaners can release chlorine gas, so never use them together. For primers and cleaning solvents, follow the product's safety data sheet, the SDS, for protective equipment, ventilation and control of ignition sources.

Sources

  1. ASTM International. (2020). ASTM C1247-20, Standard test method for durability of sealants exposed to continuous immersion in liquids. https://store.astm.org/c1247-20.html
  2. Colin, X., Audouin, L., Verdu, J., Rozental-Evesque, M., Rabaud, B., Martin, F., & Bourgine, F. (2009). Aging of polyethylene pipes transporting drinking water disinfected by chlorine dioxide. I. Chemical aspects. Polymer Engineering & Science, 49(7), 1429–1437. https://doi.org/10.1002/pen.21258
  3. Gledhill, R. A., & Kinloch, A. J. (1974). Environmental failure of structural adhesive joints. The Journal of Adhesion, 6(4), 315–330. https://doi.org/10.1080/00218467408075035
  4. Lee, T., Rees, T., & Wilford, A. (1992). Polysulfide sealants in water-retaining structures. In Science and technology of building seals, sealants, glazing, and waterproofing (pp. 47–56). ASTM International. https://doi.org/10.1520/STP24234S
  5. Naval Facilities Engineering Service Center [NFESC]. (n.d.). Joint sealant inspection: Pools 13 and 17 (Site Specific Report SSR-2453-SHR). Defense Technical Information Center, AD1092430. https://apps.dtic.mil/sti/html/tr/AD1092430/index.html
  6. Plueddemann, E. P. (1991). Silane coupling agents (2nd ed.). Plenum Press. https://doi.org/10.1007/978-1-4899-2070-6
  7. Randazzo, S. (1992). Sealants for construction joints subjected to continuous water immersion. In Science and technology of building seals, sealants, glazing, and waterproofing (pp. 57–64). ASTM International. https://doi.org/10.1520/STP24235S
  8. Sika. (n.d.). Sikasil Pool [Product information]. Retrieved November 2026. https://nzl.sika.com/en/construction/joint-sealing/tanks-pools/sikasil-pool.html
  9. World Health Organization [WHO]. (2006). Guidelines for safe recreational water environments. Volume 2: Swimming pools and similar environments. https://www.who.int/publications/i/item/9241546808
  10. Xie, F., Zhang, T., Bryant, P., Kurusingal, V., Colwell, J. M., & Laycock, B. (2019). Degradation and stabilization of polyurethane elastomers. Progress in Polymer Science, 90, 211–268. https://doi.org/10.1016/j.progpolymsci.2018.12.003
  11. Zanni-Deffarges, M. P., & Shanahan, M. E. R. (1995). Diffusion of water into an epoxy adhesive: Comparison between bulk behaviour and adhesive joints. International Journal of Adhesion and Adhesives, 15(3), 137–142. https://doi.org/10.1016/0143-7496(95)91624-F

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.