KALTECKOREA

BlogApplication notes

Why does sealant shrink and sink as it cures?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Sealants & Damping

Applying a second layer over a sunken bead is the usual response, but if the shrinkage comes from volatiles leaving the sealant, the new layer shrinks again for the same reason. What actually lies behind it can be solvent or water leaving the bead, a joint that is too deep, an absorbent substrate, late or missing tooling, or low solids, and sometimes two or more at once.

Background

The joints around window frames and between façade panels were filled and neatly tooled, yet a few days later the surface has sunk into a hollow along the middle. Rainwater and dirt collect in the groove, and the look alone can draw complaints from the client. A bead that has thinned in the middle takes the load there first as the joint opens and closes, so the problem may not stay cosmetic. Fixing it means cutting out the cured sealant and installing again, and on a tall façade that adds the cost of putting scaffolding or a lift back up.

Sealant shrinkage after installation comes from volatile components leaving the sealant. The standard test measures that loss of volume, and the result is used to predict the appearance and shape of the cured bead and to judge how much tooling it needs (ASTM International, 2022a). Sealant made by dissolving a polymer in solvent cures as the solvent evaporates, and where the solvent can escape it shrinks as it hardens (Gibbons, 1961). So how much a bead shrinks depends on what leaves it and how much, and the shape of the shrinkage depends on how the sealant is held in place while that happens.

The sunken shape forms like this. Even after the surface has cured into a thin skin, volatiles keep leaving from below, and because the edges are held by the two joint walls, the lost volume shows up as the middle being drawn downwards. Studies on coatings likewise found that the volume of solvent lost after the film begins to solidify stays in the film as strain and stress (Croll, 1979).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: find the cure type, solids and volume change in the technical data sheet, the TDS, for the cartridge or pail that was used, and compare them with the joint width and depth, substrate, weather and tooling time on the day of installation.

Hypothesis 1: volatile loss

Water-based sealants such as water-clean-up acrylic latex, and solvent-based ones such as butyls and some acrylics dissolved in solvent, lose part of their applied volume as they cure. Because they are cheap, easy to apply and paintable, such products sometimes end up in wide exterior joints that move a lot. Picture an interior fit-out where the gap between skirting and wall was filled with a water-based acrylic sealant. On the evening it was applied, the surface sat level with the wall; by the next morning a concave groove runs along it, deepest where the gap was widest.

A water-based sealant is a latex: tiny polymer particles suspended in water. As the water evaporates, the particles move together and pack closely, are pressed out of shape, and finally lose their boundaries to form one continuous film. The process depends on conditions such as ambient temperature and humidity, surfactants, plasticisers and pigments (Keddie, 1997). The space the water occupied is simply lost, so the standard test calculates volume shrinkage from the weight lost over 28 days and the sealant's density, treating all the volatiles lost as water (ASTM International, 2022a). A solvent-based sealant hardens as its solvent evaporates from the dissolved polymer; it has its own specification and is generally formulated for joint movement of about 7.5% (ASTM International, 2022c).

Start with the TDS and label of the product left over and check the cure type. The first fork is whether it is an evaporative product that cures as water or solvent leaves, or a reactive one that cures with moisture from the air or by reaction of two parts. For a number, extrude the same product onto release film, weigh it, then weigh again over several days to see how much weight it loses. The international standard for change in mass and volume of building sealants works on the same idea, holding specimens under set conditions for a set period and measuring what has been lost (ISO, 2023).

When the trail leads to an evaporative product with a high volatile content, look first at what the joint is for. For exterior joints that move a lot or are deep, review a reactive elastomeric sealant with the supplier in place of an evaporative one. Where an evaporative product stays, as in trim gaps, fill in two passes only if the supplier allows it, letting the first layer dry well before adding the next, and set the surface height with the shrinkage in mind. If the joint is to be painted, paint only after the sealant has fully dried, so the sunken shape does not reappear under the paint.

Hypothesis 2: joint too deep

Consider this hypothesis when a deep joint was filled to the bottom with no backer, when the backer was pushed in too far, or when the gap depth varies from place to place, as between concrete panels or around window frames. Suppose that on one façade the backer ran short, so a few runs were packed deep with sealant while the rest had backer fitted properly and were filled shallow. The same product, the same day and the same applicator, yet weeks later only the deeply filled runs have visibly sunk further.

Depth matters because volatiles can leave only through the surface. Water or solvent near the bottom has to diffuse up through the sealant to get out, and the time this takes grows with the square of the thickness, so doubling the thickness makes it roughly four times as long (Crank, 1975). Meanwhile the surface cures first into a skin, and volume lost after solidification begins stays in the film as strain (Croll, 1979). A drying latex film does not dry evenly either: the boundary between solid and still-fluid regions moves sideways as it dries, and the marks of uneven drying can remain as differences in the thickness of the dried film (Routh & Russel, 1998). The deeper the joint is filled, the more volatile is still leaving under the skin late in the cure, and the longer the middle is pulled down.

Cut through a few sunken spots and look at the section. Measure the actual depth and width of the sealant and the position of the backer, and compare run by run whether the sinking grows with the depth of the sealant. There are reference values to go by. Guidance on masonry wall joints recommends that for joints about 6 to 13 mm wide the sealant depth should generally not exceed the width, and that at least about 3 mm should remain at the middle after tooling (CMHA, n.d.). If the sinking is concentrated in runs much deeper than they are wide, the weight falls on this hypothesis.

If depth is the cause, fix the backer before worrying about the fill. Press in a backer slightly larger than the joint width so that it sets the bottom of the sealant at the intended depth, and on joints of uneven depth measure each run before installation and set the backer depth to match. Runs already filled deep should not just be topped up; cut them out and reinstall, starting with the backer. The same guidance sizes closed-cell backer at about 1.25 to 1.33 times the joint width (CMHA, n.d.).

Hypothesis 3: absorbent substrate

Suspect this hypothesis when sealant went onto porous substrates such as concrete, mortar, brick or natural stone without primer, especially on a dry, sunny day with bone-dry substrate. Sinking may appear first at the edges where the sealant meets the substrate rather than in the middle, or a damp-looking band may form on the substrate along the bead. Take a site where joints between metal frames and brick and joints between metal panels were filled on the same day with the same product. The metal-to-metal joints cured evenly, but on the brick side the bead has sunk slightly along its edge, and a dark band has formed on the brick along the sealant.

Porous substrates draw in liquid that touches them by capillary force. In an experiment that used magnetic resonance to measure how fast brick takes water from freshly laid mortar, fired-clay brick extracted the water within 3 minutes and sand-lime brick over about 10, and the moisture left in the mortar depended on the suction of the brick (Brocken et al., 1998). A water-based sealant, whose liquid phase is water, can be subject to the same suction where it touches the substrate, giving its water a second way out besides evaporation. Components such as solvents and plasticisers can migrate into the substrate too, to the extent that there is a standard test for whether a sealant's fluids exude into porous stone and stain it (ASTM International, 2022b). The volume of whatever leaves can be lost first on the substrate side, and a stain may be left on the substrate as well.

Look first for a dark band or stain on the substrate along the sealant. A few drops of water on the substrate beside the joint show quickly whether it soaks in. Set joints filled with the same product side by side, those against absorbent substrate and those against non-absorbent surfaces such as metal or glass, and check whether the sinking clusters on the absorbent side. Check too whether primer was used and, if so, whether the product, amount and drying time are in the installation records.

With absorption as the likely culprit, seal the substrate first and reinstall. Follow the sealant supplier's recommendation on whether a primer is needed; some primers can be applied to damp masonry (CMHA, n.d.). Apply primer thinly and evenly at the supplier's rate, and place the sealant within the stated time. For stone finishes where staining is a concern, a staining test on that stone and sealant combination before installation can head off later disputes.

Hypothesis 4: late or no tooling

This covers working methods where a long joint is extruded end to end first and tooled later in one go, hot days and other conditions that make the surface skin quickly, and finishing work in a rush where tooling is skipped. Think of a two-person crew, one running ahead extruding the bead and the other following with the spatula. The front person is fast and the gap grows, so on the last run the spatula drags the skin into fine wrinkles. A few days later, only that run shows patches where the surface has dropped.

Tooling is more than smoothing the surface. It presses the sealant against the backer and joint walls and removes trapped air pockets, and air pockets that tooling fails to remove can expand in hot weather (Persily, 1993). Masonry wall guidance likewise holds that tooling brings sealant into intimate contact with the substrate and consolidates it, and calls for tooling to a concave shape immediately after the joint is filled (CMHA, n.d.). Pressed after a skin has formed, only the skin is pushed and wrinkled while the sealant below is not consolidated, and the surface can drop over gaps left against the walls or backer. The standard test likewise uses the shrinkage value to gauge both the shape of the cured section and how much tooling is needed (ASTM International, 2022a).

The first thing to look at is the surface texture. Fine wrinkles or torn texture in the spatula marks mean the bead was tooled after it had skinned. Cut through a sunken spot and look in the section for voids within the sealant, faces pulled away from the joint wall, and gaps between backer and sealant. From the work records or the applicators, find the interval between extruding and tooling and the temperature and humidity that day, and compare them with the tooling time or skin time given in the TDS.

The remedy starts with a shorter unit of work. Set the length extruded at a time to what can be finished within the TDS tooling time, and shorten it further on hot days when the surface skins quickly. With a two-person crew, keep the front person no more than a set distance ahead. Runs that already have voids under the skin should be cut out and reinstalled rather than patched on top. An even concave face left by tooling is the intended shape, so this hypothesis is for explaining patchy spots where the surface has dropped.

Hypothesis 5: low solids

Solids are what remains once all the volatiles have gone. Even among evaporative products, clear grades and products thinned on site with water or thinner to extrude more easily can leave less behind. Imagine the same joints on one site filled in sections with a white sealant and a clear one. Width, depth, substrate and applicator are all the same, yet the runs done with the clear product have sunk visibly deeper.

The less that remains, the smaller the volume after cure. The latex sealant specification splits this difference into types. Opaque types containing pigments or extenders may shrink by no more than 30% in volume, while clear or translucent types are allowed up to 50% (ASTM International, 2023). A wider limit for clear types means that, within the same family, they can shrink that much more. Older work on caulking compounds points the same way: solvent added for workability causes shrinkage and cracking once it evaporates if overdone, and fine limestone filler improves stability by reducing shrinkage (Gibbons, 1961).

If the TDS gives solids or volume shrinkage, start there and confirm which type of the specification the product falls under. Without that figure, the remaining share can be measured directly by weighing a sample, drying it and weighing it again, and the standard test calculates volume shrinkage from this weight loss and the density (ASTM International, 2022a). Ask the applicators whether water or thinner was mixed in, or whether product stiffened by cold was thinned in winter. Measuring the same pail before and after thinning shows the effect of dilution straight away.

Once low solids are pinned down, agree with the supplier to use a lower-shrinkage type or a reactive product where sinking would show or the joint is deep. Do not thin on site beyond what the supplier allows, and bring product stiffened by cold back to its stated storage temperature instead of thinning it. Where a clear product is a must, designing the joint shallower to allow for sinking is another option.

Finding the cause

There is no need to investigate all five hypotheses separately. Rule out first what paperwork and the eye can confirm. The cure type, solids and shrinkage type are on the TDS and label, and the substrate, primer use and tooling time can be had from the installation records and the applicators. Cutting into joints to examine sections comes next.

The first clue is where the sinking is. If everywhere a product was used has sunk evenly, look at the product side: an evaporative product with high volatile content or low solids. If the same product sank more on certain runs only, look at what differed from run to run, such as joint depth, substrate and tooling time. Where clear and opaque, or evaporative and reactive, products are mixed on one site, differences between products show fastest.

Next come the shape of the sinking and the section. An even hollow in the middle with a section much deeper than it is wide points to joint depth; sinking that starts at the edges against the substrate, with a dark band on it, points to absorption by the substrate. Fine wrinkles on the surface with voids inside the section or faces pulled away from the wall point to late or missing tooling. Keep in mind too that an even concave face made by tooling is not a defect in itself.

If that still does not settle it, run small control trials. Install side by side two joints on the same substrate differing only in backer depth, primed and unprimed faces, runs tooled immediately and runs deliberately tooled late, and different products, then measure the depth of sinking on the same day. Change only one condition at a time, or there is no telling which one made the difference. The final check is whether joints installed the corrected way still stay level after they have fully cured.

The hypotheses can overlap. A low-solids water-based product in a deep joint has more water to lose and takes longer to lose it, and if that joint is against an absorbent substrate the water has one more way out. In such cases put right first the factors that set how much is lost, product and depth, then refine substrate treatment and tooling. While product and depth stay as they are, the effect of a change in primer or tooling is buried in the large shrinkage and cannot be compared fairly.

Limits and cautions

Solids, volume shrinkage, tooling time, primer type and drying time, and suitable joint width and depth differ by product and substrate, so numeric decisions follow the product's TDS and the supplier's recommendations. Where the sealant bears directly on safety or water-tightness, as in curtain walls, waterproofing joints or structural sealant glazing, do not settle the repair on site judgement alone; get the designer and supplier to confirm. If cracking or loss of adhesion appears along with sinking, other causes besides shrinkage need investigating as well.

Safety matters too. Solvent-based sealants, primers and cleaning solvents are flammable and give off vapour, so follow the product's safety data sheet, the SDS, for ventilation, control of ignition sources and protective equipment. Indoors and in confined spaces, make sure ventilation is adequate. Wear cut-resistant gloves when cutting out cured sealant, and work at height only with fall protection in place.

Sources

  1. ASTM International. (2022a). ASTM C1241-14(2022), Standard test method for volume shrinkage of latex sealants during cure. https://store.astm.org/c1241-14r22.html
  2. ASTM International. (2022b). ASTM C1248-22, Standard test method for staining of porous substrate by joint sealants. https://webstore.ansi.org/standards/astm/astmc124822
  3. ASTM International. (2022c). ASTM C1311-22, Standard specification for solvent release sealants. https://store.astm.org/c1311-22.html
  4. ASTM International. (2023). ASTM C834-17(2023), Standard specification for latex sealants. https://store.astm.org/c0834-17r23.html
  5. Brocken, H. J. P., Spiekman, M. E., Pel, L., Kopinga, K., & Larbi, J. A. (1998). Water extraction out of mortar during brick laying: A NMR study. Materials and Structures, 31(1), 49–57. https://doi.org/10.1007/BF02486414
  6. Concrete Masonry & Hardscapes Association [CMHA]. (n.d.). Joint sealants for concrete masonry walls (TEK 19-06A). Retrieved November 2026. https://www.cmha.org/resource/tek-19-06A/
  7. Crank, J. (1975). The mathematics of diffusion (2nd ed.). Clarendon Press.
  8. Croll, S. G. (1979). The origin of residual internal stress in solvent-cast thermoplastic coatings. Journal of Applied Polymer Science, 23(3), 847–858. https://doi.org/10.1002/app.1979.070230319
  9. Gibbons, E. V. (1961). Caulking compounds (Canadian Building Digest CBD-19). National Research Council of Canada. https://web.mit.edu/parmstr/Public/NRCan/CanBldgDigests/cbd019_e.html
  10. International Organization for Standardization [ISO]. (2023). ISO 10563:2023, Building and civil engineering sealants — Determination of change in mass and volume. https://www.iso.org/standard/86193.html
  11. Keddie, J. L. (1997). Film formation of latex. Materials Science and Engineering: R: Reports, 21(3), 101–170. https://doi.org/10.1016/S0927-796X(97)00011-9
  12. Persily, A. K. (1993). Envelope design guidelines for federal office buildings: Thermal integrity and airtightness (NISTIR 4821). National Institute of Standards and Technology. https://doi.org/10.6028/NIST.IR.4821
  13. Routh, A. F., & Russel, W. B. (1998). Horizontal drying fronts during solvent evaporation from latex films. AIChE Journal, 44(9), 2088–2098. https://doi.org/10.1002/aic.690440916

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.