KALTECKOREA

BlogApplication notes

Why does exterior sealant craze and crack on the surface?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Sealants & Damping

Putting the cracks down to age and refilling with the same product is the usual response to crazed exterior sealant, but crazing means the surface has hardened and weakened, so if the conditions behind it remain, the new sealant tends to craze again. What actually lies behind it can be surface oxidation by UV and ozone, a less durable polymer, lost plasticiser, repeated movement under large temperature swings, or cleaners and air pollutants, and two or more can act together.

Background

An inspection of exterior joints a few years after installation sometimes finds the sealant surface split into fine cracks, like a dried-out paddy field. Pressed with a finger, it has lost its original soft give, and in places the cracks have deepened and opened into the body of the joint. Surface crazing is easy to dismiss as cosmetic, but as the cracks deepen, rain and wind get into the joint and can lead to leaks indoors, wet insulation and corrosion of metal behind the panels. Resealing a facade needs a cradle or scaffold, so the cost and time of access tend to outweigh the material.

Exterior joint sealant is a rubber-like material that closes the gap by stretching and squeezing as the building moves, and its surface takes sunlight, air, water and temperature change all at once. In laboratory tests, cyclic movement, temperature, humidity and UV each played a large part in sealant degradation, and together they amplified one another (White et al., 2012). The sealant test standard likewise measures weight loss after heat ageing, cracking, and chalking, the powder that rubs off the surface, and treats cracking and chalking as signs linked to a short service life (ASTM International, 2022a).

Crazing signals that the skin has hardened and weakened, so unless the cause of that hardening is found, the same thing happens again in the resealed joint. The skin hardens by two main routes: outside agents such as sunlight, ozone and cleaners alter the polymer chains, or the ingredients that kept the sealant soft leave it. On top of that, repeated movement under large temperature swings pulls on the hardened skin and opens the cracks.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: gather the orientation and location of the crazed joints, the year of installation, the product and the cleaning records, and compare the use and movement class in the sealant's technical data sheet, the TDS, with the actual joint conditions.

Hypothesis 1: UV and ozone oxidation

The longer a joint sits in the sun, the higher this hypothesis ranks. That means joints on south and west walls, around sloping roofs and between metal panels that heat up in the sun, and it deserves closer attention for organic sealants rather than silicone. Say you walk round a building sealed in one year with one product. The joints on the sunny south wall are covered in crazing, while those on the shaded north wall are still smooth and keep their sheen.

Sunlight is a main agent of degradation in exterior joint sealant, so the accelerated weathering test for sealants alternates UV and water and then checks the specimens for cracks (ASTM International, 2023). UV breaks polymer chains, and the broken ends react with oxygen in the air, so the surface oxidises first. In tests that exposed an aromatic polyurethane to UV, carbonyl groups, the product of oxidation, increased with time and the colour yellowed with them (Rosu et al., 2009). On mock-ups left outdoors near Chicago for about 30 years, the polyurethane sealants developed surface crazing, and the authors judged that facing south at about 30 degrees from horizontal had accelerated the weathering (Chin et al., 2022).

Ozone attacks the surface by another route. It reacts with carbon double bonds left in rubber chains, cuts the chains and cracks the surface wherever it is stretched (Layer & Lattimer, 1990). That is why the ozone cracking test for rubber exposes specimens under surface tensile strain to air of set ozone concentration (ASTM International, 2025b). For a formulation whose chains still carry double bonds, a surface held in extension while the joint is open in winter and meeting ozone is in exactly that condition.

Begin by comparing joints of the same product side by side across orientations. If crazing gathers on sun-facing walls and is sparse on shaded ones, the weight shifts to this hypothesis. Cutting a thin section at a crazed spot shows whether the cracks stay in the skin or run into the body, and rubbing the surface with a finger shows whether white powder comes off. That chalking is a sign of degradation the standard test checks alongside cracking (ASTM International, 2022a).

Where oxidation is concentrated on sun-facing walls, one option while the cracks stay in the skin and the body is still elastic is to record the condition with photographs and keep watching. If the cracks have reached the depth of the joint, remove the sealant and reseal, and ask the supplier whether the new product has accelerated weathering data from alternating UV and water. Where ozone levels are high, request ozone cracking results as well. When resealing, prepare the substrate left after removing the old sealant and prime it as the standard guide sets out (ASTM International, 2025a).

Hypothesis 2: less durable polymer

Sealants are made from many polymers, among them silicone, polyurethane, polysulphide, silicone-modified organics and acrylic, and even in the same exterior joint they differ in how well they stand up to sunlight and movement. When a sealant chosen because it had to be painted, because it was cheap, or because an interior product was left over on site has gone into a facade, the polymer type is worth suspecting first. Take a building where only some window perimeters were refilled with a different sealant during repairs. A few years later, on the same wall, the original joints are unchanged while only the refilled ones show surface cracking.

Each polymer has its own weak point. In the roughly 30-year exposure above, the polyurethane sealants showed surface crazing and some softening, while ingredients from the silicone sealants migrated into the adjacent granite and stained it (Chin et al., 2022). In a year of alternating UV exposure and thermo-mechanical movement, most silicone-modified organic sealants showed limited durability in exterior joints, mainly because of poor UV resistance. In the same test, newer formulations with good UV resistance recovered poorly after compression at high temperature (Longo & Vandereecken, 2010). So no one type wins in every condition; what decides crazing is whether the type chosen suits the sunlight and movement the joint receives.

The clue lies in the paperwork. Find the product used in each joint in the as-built or repair records, and see whether the TDS lists exterior joint use, a movement class and weathering test results. Without records, take small samples from crazed and sound joints and compare colour, smell and hardness, and if needed send them to a laboratory with infrared spectroscopy to identify the polymer.

If the type was wrong, do not refill the same joint with the same product. Choose a new product classed for exterior joints, with data showing that it did not crack when bent cold after accelerated weathering (ASTM International, 2023). Remove the old sealant rather than leaving it in place, and confirm with the supplier that the new product, the substrate and the primer suit one another before sealing.

Hypothesis 3: lost plasticiser

Some formulations contain plasticisers or oils so that the sealant stays soft and extensible after cure. These ingredients leave little by little when heated, so look at this hypothesis between dark metal panels that get hot in the sun and on stone or concrete substrates that draw them in. Picture a joint between sun-facing dark stone panels after a few summers. It has become so hard that a fingernail barely dents it, and along its edges the stone carries a dark band, as if oil had soaked in.

A study of plasticiser loss from plastic and rubber products describes it in two steps: plasticiser inside diffuses to the surface, then evaporates from the surface into the air, and the slower of the two sets the overall rate (Wei et al., 2019). The sealant test standard holds that durability can suffer when ingredients critical to performance evaporate at high temperature, and it measures weight loss after heat ageing (ASTM International, 2022a). An early guide to caulking compounds notes that when oils and solvents volatilise the material hardens early and loses flexibility, and that over-thinned compounds can shrink and crack once the solvent has gone. The same guide observes that caulks tend to harden with time, their hardness usually rising a little each year (Gibbons, 1961). A sealant that stretches less then cracks from the surface when the joint opens.

Hardening is easy to confirm by measurement. Compare crazed joints with joints in shade using a rubber durometer, and if possible with a fresh sample of the same product. Check also whether the joint section has shrunk into a concave profile. A dark band on the substrate at the edges may be a trace of ingredients moving into it, and a case has been reported in which plasticiser migrating from silicone sealant left permanent stains on adjacent granite (Chin et al., 2022). A removed sample can be weighed before and after heating in a laboratory to estimate how much volatile content it still holds.

Ingredients that have left cannot be put back by treating the surface, so plan replacement. When choosing a new product, ask the supplier for weight loss and cracking results after heat ageing, and examine them closely for joints that get hot, such as those between dark panels. On stone substrates, choose a product with substrate staining test data, and build the joint to its design depth.

Hypothesis 4: thermal cycling

The members on either side of a joint grow when hot and shrink when cold, so the sealant between them is squeezed by day and stretched by night, with a larger swing across the seasons. Large metal or glass panels, dark finishes, regions with wide daily temperature ranges and joints built narrower than designed all increase the movement the sealant has to take. On a factory facade clad in wide aluminium panels, the crazing may sit not all over the building but in the vertical joints between the largest panels. On a cold morning the open cracks are plainer than at midday.

Joint movement is calculated from member length, thermal expansion of the material and the range of surface temperature, and joint width is set so that this movement stays within the share the sealant can take (ASTM International, 2022b). The durability test for sealants likewise takes specimens through water and heat, then repeatedly compresses them hot and extends them cold to see whether adhesion and cohesion hold (ASTM International, 2022c). Sealant stiffens at low temperature, and that is exactly when the joint opens widest and pulls hardest on a hardened skin. The accelerated weathering test bends specimens cold to look for cracks because weather combined with extension can degrade sealant more severely (ASTM International, 2023).

Measuring the actual movement comes first. Measure joint width and sealant depth with a tape and a depth gauge, and measuring the same spots once in summer and once in winter shows how far the joints really move. Compare these figures with the design movement calculation and the movement class in the TDS. Mark on an elevation whether crazing gathers at large panels, dark faces and joints far from fixing points, and see whether it coincides with the joints that move most.

If movement exceeds what the sealant can take, putting the same product back into the same width only cracks the same joints again. Review with the designer whether the joints can be widened or a product with a higher movement class used, and set sealant depth and shape with backer rod. Keep the temperature during application within the range the TDS sets.

Hypothesis 5: cleaners and pollution

For buildings whose facades and glazing are washed regularly, sites that use strong acid or alkaline cleaners to lift stains or efflorescence from stone, and joints in cities and industrial areas where ozone often rises on hot, sunny days, weigh up what reaches the joint from outside. On a shopping building washed every year, the crazing may not be even across the facade but gathered in lower joints along the streaks where cleaning solution ran down. There the surface is rough and differs in colour from its surroundings.

Cleaners do not always harm sealant. One sealant manufacturer states that many cleaning solutions, among them hydrogen peroxide, sodium hypochlorite, alcohols and citric acid, are generally compatible with fully cured sealant, yet advises against prolonged or continuous exposure and asks for rinsing as the instructions direct (Pecora, 2020). The standard test that immerses sealant in liquid does not, in its standard form, test the effect of acids or alkalis, so finding out what an actual cleaner does means a test modified by agreement between the parties (ASTM International, 2020).

On the air side, look at ozone. Ground-level ozone forms when nitrogen oxides and volatile organic compounds from vehicles and factories react in sunlight, and it tends to rise on hot, sunny days in cities (EPA, n.d.). Ozone progressively damages materials such as rubber, plastics and paint, degrading both function and appearance (CARB, 2016). Even with one product, joints in places where ozone often runs high meet harsher air.

Start by finding the cleaning records. Note which cleaner was used at what strength, how long it stayed on the joints and whether they were rinsed, and see whether the damaged joints line up with the paths the solution ran down. Comparing them with joints on faces that are never washed, or under eaves, brings out the difference. If a cleaner is suspect, soak or coat specimens of the same sealant in it and compare their hardness and surface with fresh specimens.

When the evidence leans towards cleaners, change the cleaning method first. Ask the sealant supplier about compatibility before switching cleaners, trial them on a small area first, shorten dwell time and rinse thoroughly. Where a strong cleaner is unavoidable, mask the joints before work. When resealing in areas where ozone often runs high, give priority to types with ozone and UV exposure data.

Finding the cause

Five hypotheses do not need five investigations at once. Rule them out starting with what can be seen on a walk round and what is already on paper. Joint orientation and location, year of installation, product and cleaning records can be gathered quickly, and taking samples for a laboratory comes after that.

The first clue is where the crazing gathers. Crazing on sun-facing walls with the shaded walls sound points to UV and ozone oxidation; crazing only in joints refilled with another product during repairs points to the polymer type. Crazing concentrated in joints that move most, between large panels or on dark faces, points to thermal cycling, and crazing that follows the run of cleaning solution points to cleaners. A dark band at the joint edges with a hard, shrunken sealant turns attention first to lost plasticiser.

Next comes the section. Cut a crazed spot to see whether the cracks stay in the skin or reach the depth of the joint, and compare the hardness of skin and body. A hardened skin alone puts the weight on outside agents changing the surface; a body hardened evenly throughout puts it on ingredients having left. Since plasticiser loss runs at the pace of the slower of diffusion and evaporation (Wei et al., 2019), the skin alone may be depleted, so do not decide on one section.

If that still does not settle it, bring in a laboratory. Put removed samples and fresh samples of the same product through heat ageing and compare weight loss, cracking and chalking, and compare candidate replacements by their accelerated weathering results. A laboratory weathering test should reproduce the degradation mechanism and failure mode seen outdoors (Wypych et al., 2004), so also check that the crazing pattern from the test matches the one on the building.

The hypotheses can overlap. Cyclic movement, temperature, humidity and UV each play a large part in degradation and amplify one another when combined (White et al., 2012). A skin hardened by sunlight splits first when the joint opens on a cold day, and a sealant that has lost plasticiser is weaker under the same movement. In such cases, first stop the causes still at work, such as the cleaning method, then reseal with joint design and product corrected together, because fixing only one leaves the other conditions to harden the new sealant.

Limits and cautions

Suitable movement class, joint width and depth, and replacement interval differ by product, member and local climate, so numeric decisions follow the product's TDS and the designer's calculations. Where cracking appears in structural sealant that holds glass or in curtain wall joints, do not overcoat on site judgement; get the facade designer and the manufacturer to confirm. If insulation or panel fixings behind the joint are already wet or corroded, replacing the sealant will not finish the job, so have a facade specialist inspect it.

Safety matters too. Facade inspection and repair is work at height, so do it only with fall protection and a work plan in place. For cleaners, primers and sealants, follow each product's safety data sheet, the SDS, for protective equipment and ventilation, and take care against cuts when cutting out old sealant with a knife.

Sources

  1. ASTM International. (2020). ASTM C1247-20, Standard test method for durability of sealants exposed to continuous immersion in liquids. https://store.astm.org/c1247-20.html
  2. ASTM International. (2022a). ASTM C1246-17(2022), Standard test method for effects of heat aging on weight loss, cracking, and chalking of elastomeric sealants after cure. https://store.astm.org/c1246-17r22.html
  3. ASTM International. (2022b). ASTM C1472-16(2022), Standard guide for calculating movement and other effects when establishing sealant joint width. https://store.astm.org/c1472-16r22.html
  4. ASTM International. (2022c). ASTM C719-22, Standard test method for adhesion and cohesion of elastomeric joint sealants under cyclic movement (Hockman cycle). https://store.astm.org/c0719-22.html
  5. ASTM International. (2023). ASTM C793-23, Standard test method for effects of laboratory accelerated weathering on elastomeric joint sealants. https://store.astm.org/c0793-23.html
  6. ASTM International. (2025a). ASTM C1193-25, Standard guide for use of joint sealants. https://store.astm.org/c1193-25.html
  7. ASTM International. (2025b). ASTM D1149-18(2025), Standard test methods for rubber deterioration: Cracking in an ozone controlled environment. https://store.astm.org/d1149-18r25.html
  8. California Air Resources Board [CARB]. (2016). Ozone effects. Retrieved November 2026. https://ww2.arb.ca.gov/resources/fact-sheets/ozone-effects
  9. Chin, I. R., Heidbrink, F. D., & Rouse, B. K. (2022). Effects of approximately 30 years of outdoor exposure in the Chicago, Illinois, area on silicone and polyurethane sealants. ASTM STP 1633, pp. 171–194. https://doi.org/10.1520/STP163320200046
  10. Gibbons, E. V. (1961). Caulking compounds (Canadian Building Digest CBD-19). National Research Council of Canada. https://web.mit.edu/parmstr/Public/NRCan/CanBldgDigests/cbd019_e.html
  11. Layer, R. W., & Lattimer, R. P. (1990). Protection of rubber against ozone. Rubber Chemistry and Technology, 63(3), 426–450. https://doi.org/10.5254/1.3538264
  12. Longo, D., & Vandereecken, P. (2010). Relative resistance of silicone and Si-hybrid based sealants to alternating periods of accelerated weathering and thermo-mechanical movements. ASTM International symposium paper, pp. 157–164. https://doi.org/10.1520/STP48967S
  13. Pecora Corporation. (2020). Pecora joint sealant chemical compatibility: Cleaning agents, degreasers and detergents (Technical Bulletin #213). https://www.pecora.com/wp-content/uploads/pdfs/PEC-213-Pecora-Joint-Sealant-Chemical-Compatibility-Cleaning-Agents-7-7-2020-mdm.pdf
  14. Rosu, D., Rosu, L., & Cascaval, C. N. (2009). IR-change and yellowing of polyurethane as a result of UV irradiation. Polymer Degradation and Stability, 94(4), 591–596. https://doi.org/10.1016/j.polymdegradstab.2009.01.013
  15. U.S. Environmental Protection Agency [EPA]. (n.d.). Ground-level ozone basics. Retrieved November 2026. https://www.epa.gov/ground-level-ozone-pollution/ground-level-ozone-basics
  16. Wei, X.-F., Linde, E., & Hedenqvist, M. S. (2019). Plasticiser loss from plastic or rubber products through diffusion and evaporation. npj Materials Degradation, 3, 18. https://doi.org/10.1038/s41529-019-0080-7
  17. White, C. C., Hunston, D. L., Tan, K. T., & Filliben, J. J. (2012). A systematic approach to the study of accelerated weathering in building joint sealants. Journal of ASTM International, 9(5). https://www.nist.gov/node/586656
  18. Wypych, G., Kuberski, S., & Lee, F. (2004). Sealant failure morphology: The important criterion of equipment selection for weathering studies. ASTM International symposium paper, pp. 310–321. https://doi.org/10.1520/STP12571S

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.