KALTECKOREA

BlogApplication notes

Why does white sealant turn yellow?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Sealants & Damping

Re-sealing with a different white product is the usual response when white sealant yellows, but if the condition that changed the colour is still there, the new joint tends to go the same way. What actually causes the yellowing can be sunlit aromatic polyurethane, phenolic antioxidants meeting nitrogen oxides, ingredients migrating from adjoining rubber, bitumen or tape, heat, or cleaning chemicals, and sometimes two or more at once.

Background

A sealant joint that was snow white when it went in has turned ivory and then yellow a few months or years later. The change shows first where white was chosen on purpose, around window frames, between façade panels, in kitchens and bathrooms, and on the walls and floors of food plants, and building owners or end customers tend to read it as poor workmanship or a faulty product.

Discolouration is usually a matter of appearance, but the loss is not small. If the yellow has formed inside the material, cleaning will not bring the white back, so the joint is cut out and redone, and the cost and the delay tend to land on the installer or the supplier. Discolouration can also come with an adhesion problem. In a two-year study of silicone sealant bonded to bitumen-based waterproofing, discolouration did not reliably predict adhesion loss, yet more than half of the specimens in direct contact with bitumen came away at that edge (Cronin et al., 2026).

A white material looks yellow when structures that absorb blue light have formed inside it. When a polymer or an additive reacts with light, heat, oxygen or polluting gases and forms quinone-type structures with long chains of conjugated double bonds, those structures absorb the short wavelengths of visible light and what is left looks yellow. One of the quinone-type products formed when phenolic antioxidants oxidise was so strongly coloured that 5 parts per million in a polyolefin could already be seen by eye (Klemchuk & Horng, 1991). The degree of yellowing can be compared in numbers by calculating a yellowness index from colour coordinates measured with a colorimeter, and the index is compared only between specimens of the same material and similar appearance (ASTM International, 2020).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: record with photos and locations where the sealant has yellowed and where it has stayed white, confirm the base polymer and cure type in the sealant's technical data sheet, the TDS, and note the site conditions alongside, such as sunlight, heaters and engine exhaust, adjoining materials, temperature and cleaning methods.

Hypothesis 1: sunlit aromatic PU

This hypothesis comes first when an aromatic polyurethane sealant, one made with an isocyanate that carries benzene rings, has been used in outdoor joints that take direct sun. Typical cases are white or light grey products left unpainted on south- or west-facing walls, and the lighter the colour, the easier the change is to see. Take a factory façade jointed on the same day from the same lot. Joints on the south wall, which gets long hours of sun, have faded to yellow, while those under the eaves and on the north wall are still white.

Aromatic urethane structures are vulnerable to light. An aromatic polyurethane exposed for 200 hours to light above 300 nm grew steadily more yellow, the colour change tracked the rise in carbonyl groups seen by infrared spectroscopy, and the authors attributed the colour to quinone-type chromophores formed by degradation (Rosu et al., 2009). In a study of polyether urethanes made with MDI or TDI, the urethane link itself broke down under light, and more so the higher the molecular weight of the soft segment (Irusta & Fernández-Berridi, 1999). Polyurethanes made with aliphatic isocyanates, by contrast, yellow little in light and are used for coatings exposed outdoors (Chattopadhyay & Raju, 2007). So for polyurethane sealants, the choice of isocyanate decides the colour in sunlight.

Begin by comparing places from the same lot that get sun with places that do not. If the depth of yellow follows sun exposure, and a thin slice cut across the joint shows a darker colour at the sunlit face than inside, suspect light. Check the TDS and the safety data sheet for aromatic isocyanate content and for whether the product is meant to be painted, and if a colorimeter is at hand, measure and log yellowness in sunlit and shaded spots.

If light looks like the cause, changing the material at re-sealing is the real fix. For white joints left open to the sun, choose a chemistry that changes colour less in light with the supplier, and if aromatic polyurethane must stay, cover it with a paint the TDS allows so that light is kept off. One manufacturer's guidance states that the best colour stability comes from acetoxy-cure silicone and acrylic sealants (Bostik, n.d.). With several candidates, run trial joints side by side on the same wall for a season or two and compare them under real conditions.

Hypothesis 2: antioxidant meets NOx

When sealant has yellowed indoors where little light reaches, look at the air. This covers places where fuel is burnt, such as buildings heated with gas or oil heaters inside, warehouses and loading bays served by engine-driven forklifts, and underground car parks with traffic. A distribution warehouse kept shut all winter with gas-fired heaters running gives this picture. Walking round in spring, the joints on the office side are unchanged, but those inside the loading bay where the forklifts ran have yellowed, even in corners that get no light.

Many plastics and rubber products slow oxidation with phenolic antioxidants, and a sealant formulation may contain them too. These antioxidants catch the radicals that spread oxidation, but in doing so they turn into quinone-type products with conjugated double bonds, and those products raised the yellowness of polyolefins (Klemchuk & Horng, 1991). The plastics industry calls the yellowing of white polypropylene in warehouses gas fading, explains it as phenolic antioxidants turning into quinones when they meet combustion gases containing nitrogen oxides, and names forklifts and gas- or oil-fired heaters as sources (Ampacet, n.d.). Nitrogen dioxide, one of the nitrogen oxides, gets into the air mainly from burning fuel in cars, trucks, power plants and off-road equipment such as construction machinery (EPA, n.d.).

Indoor discolouration only shows its pattern when air and location are recorded together. Mark on a plan whether the yellow joints cluster near combustion appliances or vehicle routes, and whether they are darker in poorly ventilated corners. Make two cured pieces from the same lot, leave one in the suspect area and the other in an office space with no combustion appliances for a few weeks, and compare the colour; that separates the effect of the air. The textile industry has traced a large share of storage yellowing to phenolic antioxidants migrating from polyethylene and polypropylene packaging (Bangee et al., 1995), and it already has tests for this kind of discolouration: one for the potential to phenolic yellowing and one for colourfastness to the nitrogen oxides in burnt gas fumes, and both can guide a comparison of sealant specimens (ISO, 2007; AATCC, 2020).

If the air is to blame, deal with the source and the ventilation first. Review with the facilities team whether combustion heaters and forklifts can be vented outside or replaced with electric ones, and increase ventilation where indoor air stagnates. When changing sealant, ask the supplier whether the product uses an antioxidant system that discolours less where nitrogen oxides are present, and screen the candidates with the comparison test above. The plastics industry source on gas fading notes that this colour may look paler after sunlight, but the antioxidant has not been restored, so fading colour does not mean the cause has gone (Ampacet, n.d.).

Hypothesis 3: adjoining materials

If the sealant touches another material, ingredients may have migrated from it. Common partners are bitumen membranes and primers, rubber gaskets and setting blocks such as EPDM or neoprene, products containing wax, and self-adhesive tapes put on and peeled off during installation. Say white silicone sealant has been run over the edge of a bitumen membrane at the perimeter of a flat roof. A few months later a brown band starts to spread from the side touching the membrane, fading back to the original white further away from it.

Standards divide the routes into three. Contact staining forms on the surface touching the material, migration staining spreads beside and beyond the contact, and diffusion staining comes up through a light-coloured top layer, and all are especially likely under heat, pressure or sunlight (ASTM International, 2025). Sealant manufacturers' guidance likewise names bitumen, neoprene, EPDM and wax-containing products as materials whose ingredients migrate into sealant, and notes that ingredients of a self-adhesive tape's glue layer can migrate and cause yellowing after the tape is removed (Bostik, n.d.). In a study of silicone sealant bonded directly to bitumen-based waterproofing, nearly every specimen touching bitumen discoloured. Oily, low-molecular-weight hydrocarbons bled from the membrane and oxidised on the sealant surface into a cracked, carbon-rich layer; the sealant's own colour did not change, and formulations sold as non-staining did not consistently discolour less (Cronin et al., 2026).

Where the colour starts is the first clue. If the discolouration is darkest at the edge against the adjoining material and fades with distance, or follows the outline of a tape that was once there, this hypothesis is strong. Wipe the yellow surface layer with a damp cloth or pare off a thin slice to see whether the sealant beneath is white. If the partner is an accessory used with the sealant, such as a gasket, setting block or spacer, a compatibility test that checks the sealant's colour change and adhesion change after heat and ultraviolet exposure can screen it in advance (ASTM International, 2023).

If it came from the adjoining material, keeping the two apart is the answer. Where silicone has to meet a bitumen-based material, a layer that physically separates them, such as a polyethylene-faced membrane or sheet-metal flashing, is recommended, and destructive adhesion testing once the sealant has first cured belongs in quality control. Adhesion loss may not show up straight away, or even within the first several weeks (Cronin et al., 2026). Match gaskets and setting blocks to materials whose compatibility the sealant supplier has confirmed, and do not leave tape on faces the sealant will touch for long.

Hypothesis 4: heat ageing

Suspect heat when something hot sits close to the joint. Typical places are where hot water or steam pipes pass through a wall, around ovens and dryers, behind light fittings, and on dark metal roofs and panels heated by the sun, and the discolouration may follow equipment running hours more than the season. The penetration where a dryer exhaust duct leaves through a wall is one example. The joint around the duct has turned deep yellow from the side nearest the duct, while the same joint a hand's width away is still white.

Heat works by speeding up the other causes. Chemical reactions run faster as temperature rises, so in hot places polymer oxidation is brought forward, and the coloured quinone-type products that form when phenolic antioxidants catch radicals to stop that oxidation build up faster too (Klemchuk & Horng, 1991). Staining by ingredients migrating from adjoining rubber also happens more readily under heat (ASTM International, 2025). Where a joint takes both sun and heat, as between dark panels sealed with aromatic polyurethane, breakdown by light and oxidation by heat go on at the same time.

Measuring surface temperature is the quickest check. With the equipment running, measure the temperature of the yellowed and the white areas with a contact or infrared thermometer and compare it with the service temperature range in the TDS. Photograph whether the depth of colour fades step by step away from the heat source, and put one cured piece from the same lot in an oven at that temperature and another at room temperature; comparing them after a few weeks shows the effect of heat alone.

Reduce the heat, or move to a material that tolerates it. Fit insulation or a heat shield to pipes and ducts to lower the temperature reaching the joint, and review the detail to see whether the joint can sit even a little further from the source. If the temperature cannot come down, give the measured surface temperature to the supplier, choose a product whose service range covers it, and confirm the choice with the same oven comparison.

Hypothesis 5: cleaning chemicals

If the yellow joints are concentrated where cleaning is frequent, cleaning may be the cause. This covers kitchens, bathrooms, food and drink plants and hospitals, where chlorine bleach or disinfectants, strong alkaline or acid cleaners, or solvent-soaked cloths are used daily. Soapy water used to tool the joint during installation belongs in the same group. Picture the hygiene area of a food plant, sprayed with a chlorine disinfectant at every end-of-day clean. On the vertical joints between wall panels, the lower part where wash water runs down has faded to yellow, and the upper part, which cleaning barely reaches, has stayed white.

Sealant manufacturers' guidance on discolouration lists liquids containing acid or alkaline ingredients and vapours from detergents, chemicals and solvents as causes of yellowing, and puts the soapy water applicators use to tool joints and cigarette smoke on the same list (Bostik, n.d.). Chlorine bleach is a strong oxidiser, so it can oxidise polymers or additives into the same kind of coloured structures described above. Cleaners touch the same spot again and again every day, so a change too small to see at once builds up over months, and if the surface roughens a little with each clean, dirt clings more easily as well.

Look at the boundary between cleaned and uncleaned areas. Check whether the edge of the discolouration matches the height wash water reaches or the area the disinfectant is sprayed on, and gather the name, concentration, rinsing practice and frequency of each cleaner together with its safety data sheet. Then soak cured pieces from the same lot in the actual cleaner for a set time and rinse, repeat the cycle, and compare their colour with pieces soaked in water only. Also look in the installation records for whether soapy water was used during tooling.

Where the cleaner cannot change, cut the contact time and match the material to the cleaner. Keep cleaners at their set concentration and rinse with clean water after the specified dwell time so nothing stays on the joint. If hygiene rules require the cleaner as it is, give its name and concentration to the supplier, choose a sealant with confirmed chemical resistance to it, and check the candidates with the soak comparison above. At installation, tool joints by the method the supplier recommends rather than with soapy water.

Finding the cause

There is no need to test all five hypotheses at once. Rule them out in turn, starting with what can simply be seen. Adjoining materials and cleaning areas can be checked on one walk round the site, and sunlight and heat sources are quickly recorded with photos and a thermometer. Indoor air needs a comparison over several weeks, and the material's composition needs supplier data and tests, so they come later.

The shape of the discolouration says a lot. Yellowing only on faces that get sun points to light breaking down aromatic polyurethane, and yellowing that reaches even dark indoor corners but clustered near combustion appliances or vehicle routes points to nitrogen oxides and antioxidants. A band that started at the edge against an adjoining material points to migrating ingredients, a gradient fading away from a heat source points to heat, and a boundary that stops at the height wash water reaches points to cleaning chemicals.

Next, see where the yellow actually is. If a mild detergent and water take the colour off, it is surface dirt rather than discolouration, and field investigations have reported that silicone sealants tend to pick up dirt more, and faster, than polyurethanes (Chin et al., 1996). If a thin slice shows yellow only at the surface, think of a reaction at the surface or a layer deposited on it; if it is yellow throughout, think of a change in the whole material. A stain spreading into the stone or concrete beside the joint may be ingredients seeping out of the sealant, and a sealant's potential to stain porous stone is tested separately (ASTM International, 2022).

If that still does not settle it, run a control test with cured pieces from the same lot. Place one piece each by a sunny window, near a combustion appliance, on rubber or bitumen, in an oven at service temperature and in the actual cleaner, with one more piece given no condition at all. Give each piece only one condition, or there is no telling what changed the colour, and after a few weeks compare yellowness measured with a colorimeter between pieces of the same material. The job is done when, after the cause is fixed, the yellowness of the new joint stays close to its starting value for more than a season.

The hypotheses can overlap. In joints between dark panels that take the sun, light and heat act together, and heat also hastens migration from adjoining materials. Even indoors, combustion gases and cleaner vapours can share one space. In such cases, put right the conditions that can be changed by hand, the adjoining materials and the cleaning method, and then look again at light, heat and air, because while a removable cause is still there, the share of the others cannot be judged fairly.

Limits and cautions

Service temperature range, paintability, chemical resistance and acceptable adjoining materials differ by sealant formulation, so decisions follow the product's TDS and confirmation from the supplier. The phenolic yellowing and burnt gas tests are textile standards and serve only as a comparative reference for sealants, and results from accelerated laboratory tests do not directly predict results on site. Where discolouration appears against bitumen-based materials or in a weatherproofing joint, check adhesion as well as colour.

Safety matters too. For cleaners and solvents, follow the product's safety data sheet, the SDS, for protective equipment and ventilation, and never mix chlorine bleach with acid cleaners or products containing ammonia. Wear cut-resistant gloves when slicing or cutting out sealant with a knife, and inspect joints at height only from proper access with fall protection. Combustion exhaust building up indoors is a health issue before it is a sealant colour issue, so share it with the facilities team straight away.

Sources

  1. American Association of Textile Chemists and Colorists [AATCC]. (2020). AATCC TM23-2015e(2020), Test method for colorfastness to burnt gas fumes. https://members.aatcc.org/store/tm23/488/
  2. Ampacet. (n.d.). Yellowing and pinking of white PE/PP. Retrieved November 2026. https://www.ampacet.com/faqs/yellowing-and-pinking-white-pe-pp
  3. ASTM International. (2020). ASTM E313-20, Standard practice for calculating yellowness and whiteness indices from instrumentally measured color coordinates. https://store.astm.org/e0313-20.html
  4. ASTM International. (2022). ASTM C1248-22, Standard test method for staining of porous substrate by joint sealants. https://store.astm.org/c1248-22.html
  5. ASTM International. (2023). ASTM C1087-23, Standard test method for determining compatibility of liquid-applied sealants with accessories used in structural glazing systems. https://store.astm.org/c1087-23.html
  6. ASTM International. (2025). ASTM D925-14(2025), Standard test methods for rubber property—Staining of surfaces (contact, migration, and diffusion). https://store.astm.org/d0925-14.html
  7. Bangee, O. D., Wilson, V. H., East, G. C., & Holme, I. (1995). Antioxidant-induced yellowing of textiles. Polymer Degradation and Stability, 50(3), 313–317. https://doi.org/10.1016/0141-3910(95)00156-5
  8. Bostik. (n.d.). Discolouration in joint sealants. Bostik Academy. Retrieved November 2026. https://www.bostik.com/australia/en_AU/bostik-academy/library/discolouration-joint-sealants/
  9. Chattopadhyay, D. K., & Raju, K. V. S. N. (2007). Structural engineering of polyurethane coatings for high performance applications. Progress in Polymer Science, 32(3), 352–418. https://doi.org/10.1016/j.progpolymsci.2006.05.003
  10. Chin, I. R., Gorrell, T. A., & Scheffler, M. J. (1996). Staining potential of sealants in/on exterior wall substrates. In Science and technology of building seals, sealants, glazing, and waterproofing: Fifth volume (pp. 169–183). ASTM International. https://doi.org/10.1520/STP16056S
  11. Cronin, K., Horton, E., Schofield, M., & Kim, S. (2026). When sealants meet waterproofing: A sticky situation. IIBEC Interface. https://iibec.org/publication-post/when-sealants-meet-waterproofing-a-sticky-situation/
  12. International Organization for Standardization [ISO]. (2007). ISO 105-X18:2007, Textiles — Tests for colour fastness — Part X18: Assessment of the potential to phenolic yellowing of materials. https://www.iso.org/standard/42097.html
  13. Irusta, L., & Fernández-Berridi, M. J. (1999). Aromatic poly(ether-urethanes): Effect of the polyol molecular weight on the photochemical behaviour. Polymer, 40(17), 4821–4831. https://doi.org/10.1016/S0032-3861(98)00708-3
  14. Klemchuk, P. P., & Horng, P.-L. (1991). Transformation products of hindered phenolic antioxidants and colour development in polyolefins. Polymer Degradation and Stability, 34(1–3), 333–346. https://doi.org/10.1016/0141-3910(91)90127-D
  15. Rosu, D., Rosu, L., & Cascaval, C. N. (2009). IR-change and yellowing of polyurethane as a result of UV irradiation. Polymer Degradation and Stability, 94(4), 591–596. https://doi.org/10.1016/j.polymdegradstab.2009.01.013
  16. U.S. Environmental Protection Agency [EPA]. (n.d.). Basic information about NO2. Retrieved November 2026. https://www.epa.gov/no2-pollution/basic-information-about-no2

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.