Why do car-body seam sealers leak water?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Sealants & Damping

Patching the leak point with more sealer is the usual response, but if the reason the sealer failed to cover lies in the process, the next body built under the same conditions leaks again. What actually lies behind it can be a bead narrowed by robot speed, a bead broken by unsteady flow, hem air expanding in the oven, too little hem adhesive, a hem gap off design or oil left on the steel, and sometimes two or more at once.

Background

Water is found pooled under the boot floor or the floor mats of a body that has just been through the pre-delivery shower test. On the outside the seam sealer looks continuous, yet water got in somewhere. Water inside wets carpets and sound insulation and threatens electrical connectors, and water held in a seam starts corrosion in the crevice between the panels. Corrosion in the crevice beside a hem flange was strongly influenced by wetting and drying conditions, and metal loss was actually faster under conditions that let the hem pocket dry (Brady et al., 1989). Found after painting, it brings repair sealer, spot repainting and delayed delivery.

Body seam sealer covers the edges where panels overlap and the ends of hem flanges, closing the path by which water and dirt enter the seam. Closures such as doors, bonnets and boot lids are made by hemming, folding the edge of the outer panel over the inner panel, and the hem adhesive placed inside adds stiffness and corrosion protection (Atlas Copco, n.d.). Sealer is applied separately over it. The common PVC plastisol sealer is a paste of PVC powder suspended in plasticiser. Heated in the oven, the powder takes up plasticiser and swells, and the swollen particles fuse together as it hardens (Verdu et al., 2013).

There are two broad ways water gets through. Either some spot was never covered by sealer, or sealer that once covered it later cracked or came away from the panel. The first comes from application and the oven, the second from loads on the sealer and the panel surface, so the point where water entered and the state of the sealer there narrow the cause sharply.

In such cases the technical team sets up the six hypotheses below and rules them out one by one. The start is always the same: trace back from where the water appeared to the seam it came through, record the sealer there with photos and a cross-section, and compare the robot program, pump pressure and oven temperature records at the time that body was built, and the sealer's technical data sheet, the TDS.

Hypothesis 1: narrow bead at speed

This covers raising the travel speed of the sealer robot to meet line rate while leaving the flow setting unchanged, sections such as corners and curves where the robot keeps slowing and speeding up, and the period just after a program was copied from another model and edited. Take the week early in a launch when robot speed was raised a step to cut cycle time. Vision inspection passed the bead as present, yet in the shower test water seeps out along the hem edge under a rear door. In that section the sealer is visibly thinner than elsewhere and only just reaches over the hem edge.

The cross-sectional area of a bead is the amount leaving the nozzle per unit time divided by the speed at which the nozzle moves. Double the speed with the flow unchanged and the area halves, with width and height both shrinking. That is why robotic application systems control material flow, temperature, pressure and application speed together, and inline cameras check bead width, continuity and position (Atlas Copco, n.d.). A narrowed bead cannot cover both panels of a seam well enough, and the edge where the sealer stops on one panel becomes a path for water.

Measure the width and position of the sealer in the leaking section with a rule and compare them with the drawing's nominal width. Open the robot program and check whether the narrow section lines up with a speed change point or a corner. If inline vision logs width as a number, that record is the quickest evidence. Extruding a set length onto a panel and weighing it lets you compare sealer per unit length at different speeds.

When speed is shown to be the cause, flow and speed need pairing again. Raise the flow to suit the new speed, or if the system links flow to speed, check that setting and the corner compensation. Set the vision inspection limit on minimum width rather than on bead present or absent, so the same fault is caught at inspection.

Hypothesis 2: unsteady flow

Beads thin or break into dashes just after a pail or drum is changed, at the moment the pump reverses its stroke, when the first job of a shift starts through long lines that cooled overnight, and when cured residue builds up on the nozzle tip. Think of a few bodies built straight after a drum change, where the sealer line is broken here and there. One of the breaks lines up exactly with a leak in a floor seam, while the bodies before and after are fine.

The flow of a viscous fluid through a pipe is proportional to the pressure difference along it, inversely proportional to viscosity, and proportional to the fourth power of the pipe radius (Bird et al., 2002). If supply pressure dips for a moment or cold sealer is more viscous, less leaves the nozzle, and because flow follows the fourth power of the radius, a tip narrowed only slightly by residue cuts flow sharply. A pocket of air drawn into the line during a drum change leaves a gap in the bead as long as the pocket when it passes the nozzle. A review of fluid dispensing processes likewise holds that the dispensed amount depends on supply pressure, fluid properties and process conditions, so a consistent amount requires handling them together (Chen, 2009).

Pull the pressure records at the pump outlet and before the nozzle and match them with the build times of the bodies with breaks. If those bodies cluster around drum changes, shift starts or pump stroke reversals, this hypothesis gains weight. Measure the sealer temperature in the lines and at the nozzle, and look for cured residue on the nozzle tip. If there is no pressure record, fitting a gauge and logging it for one shift is the place to start.

After a drum change, define a procedure for bleeding air and an amount of first output to purge. If pressure drops at pump stroke reversal, review a pressure regulator or surge damper with the supplier, and if cold lines are the issue, add line insulation or temperature control. Set a cleaning interval for nozzles, and turn on continuity checking so vision inspection catches broken beads.

Hypothesis 3: hem air expanding

Look at this hypothesis when the hem adhesive did not fill to the hem edge and the edge was covered with sealer while a void remained inside. It applies especially when sealer that was smooth before the oven has changed after it. The scene is a door just out of the paint oven with a row of small crater-like holes in the sealer along its hem edge. A few go right through, and with a light shone in, the inside of the hem can be seen.

Trapped air at constant pressure expands in proportion to absolute temperature. By the ideal gas law, air heated from 20 to 180 °C grows to about 1.5 times its volume (Atkins & de Paula, 2014). With sealer closing the hem edge, the air builds pressure instead of volume and in the end pushes through the weakest point of sealer that has not yet hardened. An equipment supplier's account points the same way: a hem not fully filled with adhesive holds cavities and air channels, and liquid that enters them during electrocoating dries in the oven, leaving bubbles and wetting defects (Atlas Copco, n.d.). PVC sealer hardens only once the powder has taken up plasticiser and fused, and in plastisol tests the temperature of peak stiffness ranged from a little over 70 °C to a little over 150 °C depending on the plasticiser (Verdu et al., 2013). If the air escapes before then, the hole sets as it is.

Comparing the same spot on the same body before and after the oven is the surest check. If a spot that was smooth before the oven has holes after it, the weight falls on this hypothesis. Cut through the hem under a hole to see whether adhesive filled to the edge and where the void lies, and check the oven heat-up record as well.

The remedy starts with removing the void in the hem. Correct the hem adhesive amount and nozzle position so it fills to the edge, and check after hemming that adhesive shows evenly at the edge. Where voids are hard to remove altogether, review with the sealer and adhesive suppliers pre-heating the hem to cure it before sealing, or adjusting the heat-up rate.

Hypothesis 4: underfilled hem

Suspect this hypothesis when the hem adhesive was reduced or the nozzle drifted so that adhesive no longer reaches near the hem edge, all the more on parts that hem dissimilar metals, such as an aluminium outer panel on a steel inner. Sometimes sealer that was sound out of the oven shows fine cracks along the hem corners a few days later, after door open-close testing. The cracks gather near the corners rather than along the straight runs, and water seeps in along them.

Hem adhesive is the material that ties the two panels together and adds stiffness (Atlas Copco, n.d.); sealer is the material that covers the seam. Without enough adhesive the panels can move against each other inside the hem, and the sealer over the edge has to take that movement. In the oven, the movement grows if the two panels expand by different amounts as they heat. In a study that put aluminium-steel parts through simulated paint baking, gaps and distortion formed between the two metals, and shortening the joint pitch and matching the bending stiffness of the two sections were key to reducing the gap (Huang et al., 2024). Sealer not strong enough to tie the panels together can crack or come away from them when it takes such movement repeatedly.

Cut through the hem under a crack to see whether adhesive filled to the edge and whether the adhesive bead is where the design puts it. Cutting a crack-free spot on the same part and setting the two side by side shows the difference at once. Match the hem adhesive dispense records and nozzle position checks with that body's build time, and check whether the part has had a change of material combination.

Restoring the hem adhesive to its intended amount and position comes first; applying thicker sealer is no solution. For dissimilar-metal parts, review joint pitch, pre-curing of the adhesive and oven heat-up conditions with body engineering and the adhesive supplier.

Hypothesis 5: hem gap off design

Check the gap and step at the hem edge after hemming rollers or tools have been serviced or replaced, after hemming conditions have been changed, and after a change in sheet thickness or pressed-part dimensions. A typical case is leaks only from doors made in a particular hemming cell or from a particular die, though the sealer and robot program are the same. On those doors the hem edge gap is visibly wider than on others, and the sealer has sunk into it and is thin on top.

Sealer bead width and amount are set against the designed gap. A wide gap draws sealer into it so the top is thin or misses one panel, while a narrow gap with a large step leaves the bead sitting on the higher panel only, so the line to the lower one is easily left bare. Hem shape varies with the hemming process. In a study that modelled and measured roller hemming of aluminium sheet with adhesive, the force on the roller changed the roll-in of the outer panel and its surface waviness, and with adhesive present the flange waviness was slightly greater than without (Li et al., 2022). Gaps that open between the panels in the oven also change what the sealer has to cover (Huang et al., 2024).

Measure the hem edge gap and step on leaking parts with feeler gauges or a measuring device, compare them with the drawing, and set them beside the values from parts that do not leak. Trace part history to see whether a hemming cell, die or maintenance date is common to the leakers. In a section with the sealer cut away, check how far the sealer has gone into the gap.

If the gap is the cause, the fix lies in the hemming, not the sealer. Bring hemming tools and settings back to the design gap, and after maintenance measure the gap on the first part before running production. Where a gap is wide by design, reset bead width and amount so they can cover it.

Hypothesis 6: oil left on steel

Adhesives and sealers applied in the body shop often go onto steel still carrying rust-preventive oil or drawing oil from the press. Consider this hypothesis when oiling at the press has increased, when the oil type has changed, or when a new steel supplier ships with a different preventive oil. The case is parts from one lot that look unusually shiny, and on bodies built from that lot the sealer lifts cleanly off the panel when picked with a fingernail. The exposed panel shows only an oily film, with no sealer left on it.

Adhesives made to bond to oily steel clear oil from the interface by displacing or absorbing it (Debski et al., 1986). The process relies heavily on heat: in a model of rust-preventive oil diffusing into an adhesive, the oil layer had almost disappeared during the first stage of cure, as the temperature was raised to 180 °C (Ogawa et al., 1995). If there is more oil than this capacity can handle, or heating falls short, oil stays at the interface and the sealer sits on oil rather than on steel. In a study that tested bonds on oily zinc-coated steel, most failed cohesively within the adhesive, but on some coatings the PVC plastisol failed at the interface (Lundgren, 1989). Sealer with a weak interface leaves a path for water to seep in between it and the panel.

Start by peeling the sealer at the leak and looking at how it came away. A clean interfacial failure with no sealer left on the panel points to oil; tearing within the sealer, leaving sealer on both sides, points to other hypotheses. Measure oil on steel from the same lot by wiping with a clean cloth and solvent and weighing the difference, or by the supplier's method, and compare it with the range allowed in the sealer TDS. Look also for records of changes in press oil, preventive oil and oiling rate.

The first step is to confirm with the supplier which oil types and amounts the sealer tolerates, then hold the press and the steel supplier to that range. Require adhesion tests of the sealer and adhesive before any change of oil type, and set a procedure to wipe lots that exceed the range before sealing.

Finding the cause

Six hypotheses can still be cleared by ruling out first what records and the eye can settle. Robot speed and pressure records, oven temperature, and the history of hemming cells and dies can be checked without stopping the line. Cutting hems to look at adhesive or measuring oil needs samples, so it comes next.

The first clue is how the leaking bodies cluster. Leaks that keep coming from the same section after a robot program change point to speed and bead width; leaks only on the few bodies just after a drum change or shift start point to pump pressure. Leaks only on parts from a particular hemming cell or die point to the hem gap, and leaks only from a particular steel lot point to oil.

Next is the state of the sealer at the leak. A continuous but thin bead points to speed, a bead broken into dashes to unsteady flow. Crater-like holes that appeared after the oven point to hem air, and cracks that formed at the corners over time to too little hem adhesive. Sealer sunk into the gap and thin points to the hem gap; sealer that lifts cleanly off the panel points to oil.

If that still does not settle it, run control trials that change one thing at a time. Build separately a body with the original robot speed restored, one sealed after bleeding air, a part with the hem fully filled with adhesive, a part with the gap reset, and a part with the oil wiped off, and put them through the same shower test. Change only one condition at a time, or there is no telling which one worked. The final check is whether bodies built under the changed condition pass the same test one after another.

The hypotheses can overlap. A hem short of adhesive keeps a void where air pushes through the sealer in the oven, and the same hem lets the panels move so the sealer later cracks. A widened hem gap combined with a narrowed bead leaks where neither alone would. In such cases put right first what the sealer has to cover, hem adhesive and hem gap, then match bead width and pressure on that basis. While what is to be covered keeps shifting, the effect of changing sealer conditions cannot be compared fairly.

Limits and cautions

Bead width and amount, dispense pressure, oven temperature and time, hem gap and allowable oil differ by model, material, sealer and equipment, so numeric decisions follow the sealer and adhesive TDS, body engineering standards and the equipment supplier's recommendations. Interior leaks also come from door weatherstrips, bonded glass, drain holes and grommets, not only sealer, so do not conclude that the sealer is at fault before the seam the water came through has been found. Changes to hem adhesive and body structure that bear on corrosion protection and crash stiffness should not be settled on shop-floor judgement alone; get approval from body engineering and quality.

Safety matters too. For sealers, adhesives and cleaning solvents, follow the product's safety data sheet, the SDS, for protective equipment and ventilation, and keep ignition sources away from solvents used to wipe off oil. When heating PVC sealer during repair, do not exceed the stated temperature, and enter a robot cell to clean nozzles or measure beads only after the equipment is stopped and locked out.

Sources

  1. Atkins, P., & de Paula, J. (2014). Atkins' physical chemistry (10th ed.). Oxford University Press.
  2. Atlas Copco. (n.d.). Key quality factor: Hem flange bonding. Retrieved November 2026. https://www.atlascopco.com/en-hk/itba/expert-hub/articles/hem-flange-bonding
  3. Bird, R. B., Stewart, W. E., & Lightfoot, E. N. (2002). Transport phenomena (2nd ed.). Wiley.
  4. Brady, R., Yahkind, A., Kowalski, S., & Price, L. (1989). Effects of cyclic test variables on the corrosion resistance of automotive sheet steels (SAE Technical Paper 892567). SAE International. https://doi.org/10.4271/892567
  5. Chen, X. B. (2009). Modeling and control of fluid dispensing processes: A state-of-the-art review. The International Journal of Advanced Manufacturing Technology, 43(3–4), 276–286. https://doi.org/10.1007/s00170-008-1700-5
  6. Debski, M., Shanahan, M. E. R., & Schultz, J. (1986). Mechanisms of contaminant elimination by oil-accommodating adhesives. Part 1: Displacement and absorption. International Journal of Adhesion and Adhesives, 6(3), 145–149. https://doi.org/10.1016/0143-7496(86)90017-5
  7. Huang, H., Wang, Y., Lim, Y. C., Boettcher, E., & Feng, Z. (2024). Mitigation of distortion of Al/steel part under simulated paint baking condition: Experiment and numerical model studies. Journal of Manufacturing Processes, 132, 494–505. https://doi.org/10.1016/j.jmapro.2024.11.003
  8. Li, J., Zhu, W., & Wang, S. (2022). Numerical quantification model and experiment of external force on roller hemming of curved edge aluminium alloy with adhesive. Chinese Journal of Mechanical Engineering, 35(1). https://doi.org/10.1186/s10033-022-00685-5
  9. Lundgren, A. H. (1989). Volvo laboratory study of zinc-coated steel sheet-adhesive bonding properties (SAE Technical Paper 890703). SAE International. https://doi.org/10.4271/890703
  10. Ogawa, T., Ochiai, K., & Masuichi, M. (1995). Simulation analyses on the diffusion of a rust-preventing oil into an oil-accommodating adhesive. The Journal of Adhesion, 49(1–2), 83–96. https://doi.org/10.1080/00218469508009979
  11. Verdu, J., Zoller, A., & Marcilla, A. (2013). Plastisol gelation and fusion rheological aspects. Journal of Applied Polymer Science, 129(5), 2840–2847. https://doi.org/10.1002/app.39005

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.