KALTECKOREA

BlogApplication notes

Why does sprayable damping material blister and sag?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Sealants & Damping

Turning down the oven or blaming the material is the usual response when sprayable damping material blisters or sags, but blisters and sagging result from thickness, flow, baking conditions and the surface underneath acting together, so changing one alone tends to let the defect return from another direction. What actually lies behind them can be an over-thick application, water boiling during heat-up, the wrong viscosity, working temperatures outside the range or a contaminated substrate, and sometimes two or more at once.

Background

Damping material sprayed by robots onto the floor, wheelhouses and inside of the dash panel of a car body comes out of the paint oven. Bumps large and small rise across a surface that should be flat, and a few have burst into crater-like pits. On sloping faces the material has run down into wavy, curtain-like folds, and the ends of the runs have covered holes and bolt locations.

These defects do not end with appearance. Material that has run over holes and fastening points holds up assembly further down the line, and material that drops inside the oven fouls the equipment. Where blistering or running has left the thickness uneven, whether the area still reduces vibration as designed has to be checked again, and scraping off, respraying and line stops follow.

Damping material bonds to sheet steel and turns the panel's vibration energy into heat to reduce noise. Its effect is measured by bonding the material to a steel bar, vibrating it and recording the composite loss factor, which expresses how much the vibration is damped (SAE International, 2022), and there is a separate standard method for the properties of the damping material itself (ASTM International, 2017).

Sprayable damping material is used as a thick water-based coating designed to replace hand-laid pads, sprayed on and baked in the paint ovens along with the body (Hussaini, 2000). Water-based materials of this kind can cure over a wide range of conditions from room temperature to above 200°C, but curing conditions and thickness have been reported to change damping performance (Anton et al., 2017).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: record where on which bodies the defects occurred and when, collect the application thickness, material and panel temperatures, waiting time before the oven and oven temperature records for that moment, and compare them with the application and baking conditions in the damping material's technical data sheet, the TDS.

Hypothesis 1: too thick

Thickness easily overshoots when it has been raised to gain damping, where robot paths overlap and spray the same spot twice, in corners where the robot pauses as it changes direction, and where the nozzle has come closer to the panel. Sloping and vertical faces are more prone still. On one model's floor panel, the broad centre is fine, but only the edge bands and corners where robot paths overlap have blistered, and on the slopes towards the wheelhouse the material has run down along those bands.

Thickness bears on both sagging and blistering. The speed at which a wet film runs down a sloping face is proportional to the square of its thickness and inversely proportional to its viscosity, so doubling the thickness makes it run four times as fast (Jones et al., 2017). A thick film also has more water to lose and a longer path for that water to travel, so if the surface sets first, water inside is easily trapped. A study that used designed experiments to examine popping defects on a paint line likewise found that film build and the temperature of the stage that drives off water before the oven had a clear effect on popping (Prendi et al., 2008).

Measuring with a wet film gauge is quickest. Measure defective and sound spots side by side, and after baking cut a section to confirm the actual thickness. Mark the defect locations as dots on a body drawing and see whether they coincide with robot path overlaps, pause points and slopes. Compare those thicknesses with the maximum single-pass thickness in the TDS; if the defects gather only where it is exceeded, this hypothesis is strong.

If thickness is the cause, fix the robot paths first. Narrow the overlap, reduce or cut the flow in corners where the robot changes direction, and hold nozzle distance and travel speed constant. If more damping really calls for more thickness, spray it in stages within what the TDS allows, or review the material and its placement with the supplier. After changing thickness, check the damping performance again.

Hypothesis 2: boiling water

Look at this hypothesis on lines that bake water-based damping material in the paint oven, when the flash-off, the time at room temperature that drives off water before the oven, has been shortened, or when the first oven zone heats up quickly. Take the week the line speed was raised. From the moment the wait before the oven grew shorter, round bumps on the baked damping material became more numerous. Cut one open with a knife and it is hollow inside.

Water-based damping material contains a good deal of water. The bakeable damping material mentioned above was designed at 82% non-volatile content, the rest being volatile (Hussaini, 2000). When water evaporates from a drying film faster than the particles can spread back by diffusion, particles crowd towards the surface and a skin forms (Routh & Zimmerman, 2004). Observations that harsh drying at high temperature forms a skin that traps water have also been reported (Henshaw et al., 2006).

When water trapped under the skin is heated past its boiling point in the oven, it turns to vapour and expands greatly, and the pressure pushes up the still-soft skin into a blister. If the skin cannot hold and bursts, a hole or crater remains, a defect known in painting as popping (Jones et al., 2017). So with the same material, the shorter the time to drive off water and the faster the heat-up, the more blisters appear. Changing the baking temperature and time can also alter damping performance, so oven conditions have to be set with both blistering and performance in view (Anton et al., 2017).

Look at the actual panel temperature rather than the oven air temperature. Running a temperature logger through the oven on a body gives a curve of when and how fast the panel under the damping material heats up, to compare with the TDS baking conditions and flash-off time. Cut blisters open as well to see whether they are hollow. Some damping materials, however, are designed to expand on purpose; in one development the expansion was set at 1.8 times the volume (Tsuruta et al., 2006), so check the TDS first on whether evenly spread fine pores are normal.

Once boiling water is confirmed, give more time to drive off water before the oven. Review with the paint process engineer extending the flash-off, adding a low-temperature preheat zone, or making the temperature rise in the first zone gentler. If line speed leaves no room for more time, look with the supplier for a material with a wider bake window. After any change to oven conditions, confirm damping performance again with the steel bar test.

Hypothesis 3: wrong viscosity

Viscosity moves with the state of the material. Look at drums that settled in storage and were used without thorough mixing, water added to thin the material, material kept circulating through pumps and lines for a long time, material stored too long, and changes to a new lot. Think back to just after a drum change. Slopes that were fine on the last of the old drum start running from the first body on the new one, while on days when the viscosity ran high and the pressure was turned up, fine bubbles multiply on the surface.

Sprayable damping material is made to thin when pushed hard, as it is through the nozzle, and thicken again once it rests on the panel. In one development, the viscosity was tuned so this behaviour was strong over a wide range of shear rates, to keep the surface from turning uneven when sprayed through a nozzle (Tsuruta et al., 2006). If the viscosity does not recover fast enough and high enough after spraying, sagging cannot be stopped; if it is too high, flow suffers, the surface is uneven and entrained air struggles to escape (Jones et al., 2017).

Sag resistance is compared with a standard test that draws stripes of several thicknesses with a notched applicator, stands the panel up and finds the thickest stripe that does not run (ASTM International, 2018). A study that tracked particles to measure flow on vertical surfaces, though, found differences in sag length between paints the test had ranked the same (Lade et al., 2015). Use the test results as a starting point for comparison, and confirm again on the slopes of real bodies.

Viscosity is comparable only when measured by the method and at the temperature set in the TDS. Measure and log viscosity just before supply for each drum and lot, and match it against the drum, lot and position within the drum at the time the defects occurred. Review mixing and thinning records and pump circulation time as well. Spray suspect material onto test panels at the same thickness, or draw it down with a notched applicator and stand it up, and compare its running side by side with normal material.

When the viscosity log lines up with the defects, put material handling right first. Mix drums evenly according to the TDS before use, never thin beyond what is permitted, and keep the supply temperature constant. If viscosity falls during circulation, review pump and line conditions with the supplier, and set aside any lot outside the viscosity range and ask the supplier to check it.

Hypothesis 4: off-range temperature

Look at temperature when the season changes, when material comes straight from an unheated store, when supply lines heat up in midsummer, and when bodies just out of an earlier oven are sprayed before they have cooled. A line on a day when bodies reached the application area hotter than usual is one example. The surface roughens soon after spraying, slopes run even more than usual, and after baking only that day's bodies show extra blisters.

The viscosity of a coating falls as temperature rises and climbs as it drops (Jones et al., 2017). Cold material is thick, so at the same pressure less comes out or it does not spread evenly, and raising pressure and flow to make up for it easily overshoots the thickness. Warm material, or material on a hot panel, thins and runs easily. A hot panel also speeds evaporation, and when evaporation outpaces the spreading of particles a skin forms more readily (Routh & Zimmerman, 2004), so on days with hot panels sagging and blistering can rise together.

Measure temperature in three places: the material just ahead of the gun, the panel surface just before application, and the air temperature and humidity in the application area. Compare these with the working temperature range in the TDS, and check the records for whether defects cluster at a certain time of day, in a certain season, or on days when the earlier process ran late. Take panel temperature with a contact thermometer on the exact spot where the damping material will go.

If temperatures are out of range, bring material and panel back within it. Fit a heater or chiller on the supply line to hold material temperature steady, and store material in a temperature-controlled area until use. Give bodies from the earlier process a waiting zone or cooling so they are sprayed only once the panel has cooled to the temperature set in the TDS. Where conditions shift with the seasons, manage viscosity and flow settings separately for each season.

Hypothesis 5: contaminated substrate

If defects appear as spots on particular panels or locations rather than over the whole body, suspect the substrate, the surface the damping material is sprayed onto. Surfaces left with press lubricant or rust-preventive oil after incomplete cleaning, handprints, spots touched by sealer, seams holding wash water, and dust and weld spatter are the causes. This is the case where, on only a few panels and always in the same place, the material has pulled back into small round holes that expose the surface beneath. After baking, a fingernail lifts the material easily around just those spots.

For a wet coating to wet a surface evenly, the surface energy of the surface must be higher than that of the coating. Where a substance of low surface tension such as oil sits in spots, the coating cannot wet those spots, pulls back around them and leaves crater-shaped holes, and adhesion there is weak too (Jones et al., 2017). Water pooled in seams and hollows produces blisters by another route. Water trapped beneath the damping material turns to vapour in the oven and pushes up the film above by the same principle described earlier, except that this time the pressure comes from the bottom rather than from within the film.

Run a water-break test on the panel before application. A standard method judges an oily film by whether the water film stays continuous when the panel is wetted and held upright, or breaks up and beads in places; it is a qualitative, pass or fail test (ASTM International, 2021). Lift a blister to see whether the surface below is oily or wet, and check whether defect locations coincide with a press lot, a manual handling step or seams where water pools. Recording blister size and density as grades against standard pictures allows comparison before and after improvement (ISO, 2016).

If the water film breaks or the surface under a blister is oily, close off the routes contamination takes. Check oil quantity and cleaning condition of the steel together with the upstream processes, have operators wear gloves and keep their hands off damping areas, and confirm the sequence so sealer steps do not overlap damping areas. Blow out water pooled in seams before application, or let it drain through drain holes and body attitude, and confirm the effect with the water-break test after the fix.

Finding the cause

The five hypotheses are not tested all at once. Rule out first what can be measured without stopping the line. Wet thickness and the material, panel and air temperatures can be measured right in the application area, viscosity and lot records are in the material logs, and oven conditions are on the temperature logger. Substrate contamination shows quickly with a water-break test, while control trials that make and bake test panels take time and come last.

The shape and location of the defects say a great deal. Blisters and sagging that gather together only at thick spots such as path overlaps and corners point first to thickness. Hollow round blisters that multiplied after the line speed went up or oven conditions changed point to water boiling during heat-up, and sagging that shifts with each drum or lot change points to viscosity. Defects that follow the season, the time of day or days when the earlier process ran late point to working temperature, and crater-like holes that recur in the same place on particular panels point to substrate contamination.

If that still does not settle it, run control trials on test panels. Spray the same material varying only thickness, only flash-off time, or only panel temperature, and onto a deliberately oiled panel and a clean one, then bake them all under the same oven conditions. Change only one condition at a time, or there is no telling what made the difference, and record results on the same basis, such as blister grade and sag length.

After fixing the cause, do not stop at appearance. If thickness or baking conditions have changed, damping performance may have changed too (Anton et al., 2017), so confirm again with the steel bar test of composite loss factor that the design value is still met (SAE International, 2022). The job is done only when blister grades and sagging are better than the records from before the fix and damping performance holds.

The hypotheses often overlap. A thick spot combined with a fast heat-up traps more water with less time to escape, so blisters rise sharply, and thin material laid thick on a hot panel both sags and blisters. In such cases, first bring thickness back within the TDS range and clean the substrate, then look at oven conditions, temperature and viscosity, because while thickness is overshooting, the effect of changing other conditions cannot be compared fairly.

Limits and cautions

Suitable application thickness, working temperature, viscosity, flash-off time and baking conditions differ by material, body and line, so numeric decisions follow the product's TDS and the standards of the supplier and the paint process. Oven conditions also affect other films such as electrocoat and topcoat, so do not change them with the damping material alone in mind; decide them with the paint process engineer, and judge damping performance on laboratory measurements.

Safety matters too. For materials and cleaners, follow each product's safety data sheet, the SDS, for protective equipment and ventilation, and wear respiratory protection during spraying so mist is not breathed in. Enter robot application areas to measure thickness or retrieve test panels only after the robot is stopped and locked out, and wear heat-resistant gloves, since bodies and test panels fresh from the oven are hot.

Sources

  1. Anton, J. T., Ley, J., Grover, I. S., & Stotera, D. (2017). The effects of cure schedule on water-based LASD loss factor and implications for prototype testing (SAE Technical Paper 2017-01-1854). SAE International. https://doi.org/10.4271/2017-01-1854
  2. ASTM International. (2017). ASTM E756-05(2017), Standard test method for measuring vibration-damping properties of materials. https://store.astm.org/e0756-05r17.html
  3. ASTM International. (2018). ASTM D4400-18, Standard test method for sag resistance of paints using a multinotch applicator. https://store.astm.org/d4400-18.html
  4. ASTM International. (2021). ASTM F22-21, Standard test method for hydrophobic surface films by the water-break test. https://store.astm.org/f0022-21.html
  5. Henshaw, P., Prendi, L., & Mancina, T. (2006). A model for the dehydration of waterborne basecoat. Journal of Coatings Technology and Research, 3(4), 285–294. https://doi.org/10.1007/s11998-006-0024-3
  6. Hussaini, A. (2000). Designing an interior applied waterborne coating for use in automotive paint shops to replace sound deadening pads (SAE Technical Paper 2000-01-1391). SAE International. https://doi.org/10.4271/2000-01-1391
  7. International Organization for Standardization [ISO]. (2016). ISO 4628-2:2016, Paints and varnishes — Evaluation of degradation of coatings — Designation of quantity and size of defects, and of intensity of uniform changes in appearance — Part 2: Assessment of degree of blistering. https://www.iso.org/standard/66399.html
  8. Jones, F. N., Nichols, M. E., & Pappas, S. P. (2017). Organic coatings: Science and technology (4th ed.). John Wiley & Sons.
  9. Lade, R. K., Musliner, A. D., Macosko, C. W., & Francis, L. F. (2015). Evaluating sag resistance with a multinotched applicator: Correlation with surface flow measurements and practical recommendations. Journal of Coatings Technology and Research, 12(5), 809–817. https://doi.org/10.1007/s11998-015-9680-5
  10. Prendi, L., Ali, A., Henshaw, P., Mancina, T., & Tighe, C. (2008). Implementing DOE to study the effect of paint application parameters, film build, and dehydration temperature on solvent pop. Journal of Coatings Technology and Research, 5(1), 45–56. https://doi.org/10.1007/s11998-007-9073-5
  11. Routh, A. F., & Zimmerman, W. B. (2004). Distribution of particles during solvent evaporation from films. Chemical Engineering Science, 59(14), 2961–2968. https://doi.org/10.1016/j.ces.2004.04.027
  12. SAE International. (2022). SAE J1637_202202, Laboratory measurement of the composite vibration damping properties of materials on a supporting steel bar. https://saemobilus.sae.org/content/J1637_202202
  13. Tsuruta, N., Noguchi, Y., & Suzuki, H. (2006). Development of a light-weight high-dampening liquid-applied sound deadener material (SAE Technical Paper 2006-01-0508). SAE International. https://doi.org/10.4271/2006-01-0508

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.