Why does welding parts with press oil on them cause spatter and porosity?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Metalworking Fluids (MWF)

Adjusting welding current or shielding gas is the usual response when oily pressed parts start to spatter and show porosity, but the gas the oil gives off as it burns and the change it makes to contact resistance stay whatever the settings. What actually lies behind it can be heavy oil residue, chlorine and sulphur in the oil, thick oil that dries slowly, skipped degreasing or contaminated electrodes, and sometimes two or more at once.

Background

A bracket fresh off the press reaches the welding cell, and the moment the arc strikes it crackles, sparks fly everywhere and the bead fills with pinhole pores. Spatter cakes on the torch nozzle and the fixture and has to be knocked off often, and porous beads are ground out and rewelded or the part is scrapped. Porosity reduces the load-bearing section of the weld, so it cannot be passed on parts where strength matters. The smoke is a problem too: at an automotive frame plant where parts were welded without the press oil being cleaned off, workers complained of skin, eye and throat irritation, and a public health agency was called in (NIOSH, 1978).

The way oil upsets a weld differs a little by process. In arc welding, oil and grease on the surface are common sources of hydrogen, and gross surface contamination produces excessive gas that is trapped in the weld pool as porosity (TWI, n.d.-a). In laser welding, evaporating oil upset the pressure balance in the keyhole, the deep cavity the laser melts into the metal, so keyhole and melt pool oscillated violently, leading to lack of fusion, porosity and blowouts where molten metal is ejected (Yang et al., 2026). Resistance spot welding generates heat from the electrical resistance where sheet meets sheet and sheet meets electrode; surface treatment can change that resistance by about an order of magnitude, and a change in resistance shifts where and how much heat is generated (Kaiser et al., 1982).

That is why processes using ordinary mineral-oil press lubricants can hardly avoid a cleaning step after forming before welding, bonding or painting, and research has gone as far as replacing the lubricant with media that volatilise without residue after forming, to do away with cleaning (Reichardt & Liewald, 2019). Put the other way round, a process that sends parts to welding without cleaning always carries the risk that oil left on the parts will upset the weld.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: pull a few parts just before welding, see where and how much oil remains, match that against where the defects appear, and compare with the press oil's technical data sheet, the TDS, its safety data sheet, the SDS, and the welding settings of the day.

Hypothesis 1: heavy oil residue

The residual amount becomes a problem when the oiling rate has been raised for a hard-to-form part, when worn oiling rolls or spray nozzles lay oil on unevenly, when oil pools inside bends or in recesses, and when oil is trapped between the faying surfaces of a lap joint. Take a part where two flanges are lapped and spot welded: welds on the flat run clean, but the ones near the bend throw sparks, and oil glistens between the faying surfaces when the part is pulled apart.

A thin film of oil may not be a problem at all; a welding research institute advises that a light coating of press lubricant or rust-preventive oil does not normally affect spot weld quality (TWI, n.d.-c). The trouble starts as the amount rises. In tests on galvanised steel sheet, sheet carrying a heavy mill oil finish shifted the acceptable welding current range lower by as much as 2,000 A and narrowed it from 1,200 A to 600 A at 12 cycles, while lightly oiled sheet showed no such change (Gedeon & Eagar, 1986). A recent study that varied the coating weight of the oil film on automotive galvannealed sheet also found that the spot welding current range narrowed as the amount rose, and under its test conditions, oil left after degreasing increased once the film exceeded about 550 mg/m² (Kim et al., 2026). With a narrower welding range, the same current leaves some welds short and pushes others into expulsion, so spatter gathers where the oil is heavy.

Residual amount comes out as a number once it is measured. Cut a coupon of set size from a part just before welding, weigh it, wipe the oil off with solvent, weigh it again, and divide the difference by the area to get oil per unit area. Measure the flat, the inside of bends and the faying surfaces separately, and see whether the porous and spattered spots coincide with where the oil is heaviest. Check oiling rolls and nozzles for wear and blockage, and compare the oiling setting with the forming specification.

The remedy is to apply only what forming needs. Cut the oiling rate and run trial forming and trial welding together, then fix an upper limit that both processes can live with. Where oil pools, put an air blow-off or wipe ahead of welding, and remove oil that would be trapped in faying surfaces before assembly. Replace oiling rolls and nozzles on a schedule so the film stays even.

Hypothesis 2: chlorine and sulphur

Consider this hypothesis when a heavy-duty press oil with extreme pressure, or EP, additives is used for deep draws or for materials that stick readily to the die, such as high-strength or stainless steel. Chlorinated paraffins and sulphur compounds have long been common EP additives. Say that after the press oil was switched to a chlorinated grade to cut forming rejects, the welding bay began to smell sharp and acrid, welders said their eyes stung, and fine cracks started to appear along the centre of the bead.

Chlorinated paraffin works so well in forming because it reacts chemically with the metal of die and workpiece to form thin films that adhere strongly to the surface (Ceron et al., 2014). That film is not a layer that runs off like oil but a reaction product bound to the metal, so when it meets welding heat, its chlorine compounds break down along with the remaining oil. Chlorinated cutting oils in welding heat can produce phosgene, an irritant gas that can flood the lungs, and in the frame plant investigation, irritation complaints made while a 35% chlorinated paraffin oil was in use fell after the content was cut below 5% (NIOSH, 1978). Sulphur does harm in another way. Solidification cracking, which forms as weld metal freezes, is associated with impurities such as sulphur and phosphorus, and welding with contaminants such as cutting oil on the parent metal increases impurity build-up in the weld pool and the risk of cracking (TWI, n.d.-b). In short, the evidence for chlorine and sulphur is clearer for harmful fumes and cracking than for porosity itself, so this hypothesis carries weight when smell and cracks appear alongside the pores.

The check opens with the oil's composition. Look in the SDS and TDS for chlorinated paraffin or sulphur compounds, and see whether the date of a grade change matches when defects rose. If the data sheets are not clear, send drum oil to a laboratory for chlorine and sulphur content. Examine welds for cracks along the bead centre with a magnifier or penetrant testing, and if there is smell and irritation, have the industrial hygienist sample the air in the welding bay.

If these constituents look responsible, choose with the supplier a chlorine-free press oil for parts that go to welding without cleaning, and if forming truly needs EP additives, put reliable degreasing ahead of welding. Before changing oil, run trial forming on the same material to make sure pickup on the die does not return. In the meantime, check local exhaust ventilation in the welding bay and log any symptoms among the welders.

Hypothesis 3: thick, slow-drying oil

Drying rate becomes the question when the time between press and welding has shortened or the oil grade has changed: when parts that used to wait about a shift after pressing now reach welding minutes later because the lines were joined, when a thin, quick-evaporating oil was swapped for a higher-viscosity one for a hard draw, or when the plant is cold in winter. Picture the first week after the lines were joined. The part is the same, yet smoke rises from the first weld, and the surface that used to feel almost dry is tacky and wet to the touch.

How much of an oil remains at welding depends not only on how much was applied but on how fast it evaporates and where it flows. An oil rich in light, volatile components loses much of itself before welding, while a viscous oil rich in heavy components leaves a film that lasts until welding heat vaporises and breaks it down all at once. Laser welding tests covered oil on the top of the upper sheet and oil between the two sheets, and in both cases evaporating oil disturbed the keyhole and caused defects (Yang et al., 2026). Flow behaviour matters as well. In an arc welding experiment comparing anti-spatter sprays applied around the joint, a free-flowing water-based product pooled heavily where the arc was extinguished and caused strong fluctuations of arc and pool, while an oil-based product held back the spread of the pool near the bevel (Ji et al., 2023). Liquid left near a weld can therefore pool in one spot and make matters worse if it flows easily, or stay put and change how the pool flows if it is viscous.

Measure drying rate as weight over time. Coat same-size panels with oil at the real application rate and weigh them straight away, after the time it takes to reach welding, and after a shift, to see how much remains. Measuring the old and new oils side by side shows the difference at once. Compare kinematic viscosity, flash point and evaporation data in the TDS, and in a cold season run the same test at shop temperature. Do not forget to check the records for whether defects rose from the date of a line change or a grade change.

If time to welding is short, choose with the supplier a grade that dries enough within that time, and confirm by trial forming that the draw still holds. If a viscous oil must stay, win back drying time before welding with an air blow or buffer storage, and move the oiling points so oil does not run into faying surfaces. Oils with a low flash point ignite more readily near welding sparks, so check the handling conditions in the SDS as well.

Hypothesis 4: skipped degreasing

Where there is a washer, the next question is whether it is actually doing its job. That is the case when the cleaning step has been dropped to save cost, when parts went straight on while the washer was down for repair or maintenance, when the cleaning solution is spent or has cooled, and when poor rinsing and drying leave water behind. Open the records for a week when the washer was bypassed for two days for maintenance, and the porosity rejects cluster in parts made on those two days, falling away once the washer runs again.

When degreasing drops out, every effect of the oil described so far reaches the weld intact. A welding research institute's guidance is to remove oil and grease from the surface at and around the weld location, and it names moisture on the workpiece surface as a hydrogen source as well (TWI, n.d.-a). Degreasing may also fail to remove everything. In the coated sheet study above, once the oil film exceeded a certain amount, more oil remained after degreasing and areas appeared where the phosphate coating did not grow (Kim et al., 2026). Residual oil can therefore cause trouble beyond welding, in pretreatment before painting. A spent cleaning solution removes less oil in the same time, and poor rinsing and drying leave water in place of oil, which becomes a hydrogen source.

The easiest judgement of a cleaned surface comes from wetting it with water. On clean metal the water spreads in an unbroken film, while where a hydrophobic film such as oil remains, the water breaks up and beads. This water-break test is standardised and can reveal very thin organic contamination, though it loses sensitivity on rough or porous surfaces (ASTM International, 2021). Match the cleaning solution's concentration, temperature and change dates and the washer pass records against the defect records, and see whether parts leaving the washer feel wet.

Once cleaning is found to be missing or weak, close the bypass first and set a fallback procedure for when the washer is down. Measure the solution's concentration and temperature at fixed intervals with rules for topping up and replacing it, and rinse and dry thoroughly. Put a floor-level cleanliness check such as the water-break test into the pre-weld inspection, and set separate cleaning conditions for heavily oiled parts.

Hypothesis 5: fouled electrodes

On a resistance spot welding line, look at the electrodes when spatter grows steadily after each tip dress. This happens when oily sheet is welded for long runs, when the dressing interval has been stretched to keep up output, and when cooling water flow has dropped. On a line where the dressing interval has been stretched, welds that are clean right after a dress start to spit from the sheet surface as the count climbs, a ring of black burnt deposit settles on the tip, and now and then an electrode sticks to the sheet.

Most of the heat generated between sheet and electrode drains into the electrode, so the tip always sits on a hot contact (Kaiser et al., 1982). On oily sheet that heat can grow. Work on coated sheet reported that welding oiled sheet at the higher currents needed for clean sheet causes expulsion and extreme overheating of the electrodes and shortens electrode life (Gedeon & Eagar, 1986). A welding research institute likewise explains that a heavy build-up of contaminant on the electrode overheats the surface and leads to surface splash and electrode sticking (TWI, n.d.-d). Put together, contamination tends to build up on the tip when the sheet is oily, and the more it builds, the more often the weld spits.

Judge the electrodes by eye and by the records. Set tips from right after a dress beside tips from when spatter had grown, and compare burnt deposit, metal pickup and how far the face has spread; keep an imprint of each tip pressed onto paper as a record of contact size and shape. Match the weld count since the last dress against when spatter and sticking began, and check the flow and temperature of the electrode cooling water. Welding wiped and oily sheet alternately with the same electrodes separates a problem that starts at the electrode from one that starts at the sheet.

With the electrodes clearly implicated, bring the dressing interval forward of the weld count at which defects start to rise. Tips mushroom or flatten as they wear, changing the contact area and with it the weld quality; dressing is still timed mainly by experience, and a method that reads the change in electrode length from process data to time it has been proposed (Mathiszik et al., 2021). Where possible, time dressing from such process data. Hold cooling water flow and temperature within set ranges. Electrodes still foul quickly on heavily oiled sheet, so do not rely on electrode care alone; correct the residual oil amount and the cleaning at the same time.

Finding the cause

Before measuring all five, map where the defects fall. If porosity and spatter cluster where oil collects, inside bends, in recesses and at faying surfaces, look at residual amount, viscosity and drying rate. If they appear evenly over the whole part and coincide with days the washer was down, look at degreasing first. In spot welding, defects that are fine just after a dress and rise with weld count point to the electrodes, and an acrid smell together with centreline cracks points to constituents such as chlorine and sulphur.

Next come the numbers that are easy to collect. Oil per unit area, the water-break test, washer records and weld count since the last dress can all be gathered within a day. Oil composition analysis and the weight-over-time test take longer, so they come after.

If the numbers still do not settle it, a control trial gives the quickest answer. Wipe a few parts from the same lot with solvent, weld them under the same settings, and compare defect counts with unwiped parts. If the wiped parts come out clean, the cause lies with the oil; if defects remain even after wiping, look separately at welding settings, gas and material. Then try freshly dressed electrodes, try welding parts held back for a shift, and compare with parts that went through the washer. Make one change at a time, or the result cannot be read.

The final check is to carry on normal production in the corrected state and count porosity rejects, spatter cleaning frequency and welds between dresses on the same basis as before. The job is done only when improved figures hold for several days.

The hypotheses can also link like a chain. A high oiling rate combined with skipped cleaning leaves more oil, and that oil fouls spot welding electrodes quickly, so spatter climbs again. However often the electrodes are dressed, it will recur while the oil stays, so put right the front of the chain first, the amount of oil and the cleaning, and then reset the dressing interval and welding settings.

Limits and cautions

Acceptable oil amount, cleaning conditions, welding current and dressing interval differ by material, coating, sheet thickness and welding process, so numeric decisions follow the press oil's TDS, the welding procedure and the equipment supplier's guidance. The test figures cited come from the materials and conditions of each study and should not be carried over as they stand. Do not accept welds that carry strength or safety on appearance alone; confirm them with the specified non-destructive and destructive tests.

There are safety points as well. Fumes from welding oily parts carry the oil's breakdown products, and chlorinated oils can give off irritant gases such as phosgene, so provide local exhaust ventilation and have the air measured where needed (NIOSH, 1978). Follow the SDS of degreasing solvents and cleaners for protective equipment, ventilation and ignition control, and keep oily rags and solvents away from welding sparks.

Sources

  1. ASTM International. (2021). ASTM F22-21, Standard test method for hydrophobic surface films by the water-break test. https://store.astm.org/f0022-21.html
  2. Ceron, E., Olsson, M., & Bay, N. (2014). Lubricant film breakdown and material pick-up in sheet forming of advanced high strength steels and stainless steels when using environmental friendly lubricants. Advanced Materials Research, 966–967, 219–227. https://doi.org/10.4028/www.scientific.net/AMR.966-967.219
  3. Gedeon, S. A., & Eagar, T. W. (1986). Resistance spot welding of galvanized steel: Part I. Material variations and process modifications. Metallurgical Transactions B, 17(4), 879–885. https://doi.org/10.1007/BF02657151
  4. Ji, A., Zhang, L., & Peng, G. (2023). Influence analysis of anti-spatter spray on welding process and weld properties. Journal of Physics: Conference Series, 2541(1), 012019. https://doi.org/10.1088/1742-6596/2541/1/012019
  5. Kaiser, J. G., Dunn, G. J., & Eagar, T. W. (1982). The effect of electrical resistance on nugget formation during spot welding. Welding Journal, 61(6), 167s–174s. https://eagar.mit.edu/publications/Eagar026.pdf
  6. Kim, J.-Y., Jung, H.-Y., Yook, W., & Yoon, S.-C. (2026). Interrelated behavior of friction, interfacial electrical resistance, and phosphate reactivity on automotive GA-coated steel sheets as a function of lubricant protective film coating weight. Surfaces, 9(3), 63. https://doi.org/10.3390/surfaces9030063
  7. Mathiszik, C., Köberlin, D., Heilmann, S., Zschetzsche, J., & Füssel, U. (2021). General approach for inline electrode wear monitoring at resistance spot welding. Processes, 9(4), 685. https://doi.org/10.3390/pr9040685
  8. National Institute for Occupational Safety and Health [NIOSH]. (1978). Health hazard evaluation determination report No. 78-89-550: The Budd Company, Red Lion Plant, Philadelphia, Pennsylvania. https://doi.org/10.26616/NIOSHHHE7889550
  9. Reichardt, G., & Liewald, M. (2019). Investigation on friction behaviour of deep drawing radii using volatile media as lubricant substitutes. Procedia Manufacturing, 29, 193–200. https://doi.org/10.1016/j.promfg.2019.02.126
  10. TWI Ltd. (n.d.-a). Defects/imperfections in welds: Porosity. Originally published in Connect, 1999. Retrieved November 2026. https://www.twi-global.com/technical-knowledge/job-knowledge/defects-imperfections-in-welds-porosity-042
  11. TWI Ltd. (n.d.-b). Defects: Solidification cracking. Originally published in Connect, 1999. Retrieved November 2026. https://www.twi-global.com/technical-knowledge/job-knowledge/defects-solidification-cracking-044
  12. TWI Ltd. (n.d.-c). Do I need to clean the metal surfaces before making resistance spot welds? Retrieved November 2026. https://www.twi-global.com/technical-knowledge/faqs/faq-do-i-need-to-clean-the-metal-surfaces-before-making-resistance-spot-welds
  13. TWI Ltd. (n.d.-d). How can I avoid surface splash or electrode sticking in resistance spot welding? Retrieved November 2026. https://www.twi-global.com/technical-knowledge/faqs/faq-how-can-i-avoid-surface-splash-or-electrode-sticking-in-resistance-spot-welding
  14. Yang, F., Ardic, C. E., Kodera, S., Saravanapavan, T., Schmidt, L., Römer, F., & Bergmann, J. P. (2026). Acoustic emission-based monitoring of oil contamination during laser beam welding. Procedia CIRP, 143, 463–468. https://doi.org/10.1016/j.procir.2026.07.096

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.