Filtering the oil or topping it up with new oil is the usual response when transformer oil darkens and runs hotter, but filtering only removes particles already formed, and while the conditions that oxidise the oil remain, sludge builds up again. What actually lies behind it can be spent oxidation inhibitor, oxygen reaching hot oil, copper speeding oxidation, excess moisture, overloading, or oxidation products that drop out once the oil can hold no more, and often two or more at once.

Background

The load has been much the same for years, yet the transformer's top-oil temperature creeps up each year and the cooling fans run more often than they used to. A thermal camera picks out a few radiator tubes that are noticeably cold, and oil drawn from the bottom valve is dark brown and cloudy. When sludge formed in the oil settles on windings, insulation and cooling surfaces, the path for heat narrows, so the temperature rises slowly at the same load, and that heat in turn speeds the ageing of the paper insulation and shortens the transformer's life considerably (USBR, 2003). A transformer is costly and slow to repair, so one failure can stop a whole plant or substation, and insulation failure is counted among the main causes of transformer failure (Elele et al., 2022).

Transformer oil insulates the windings and carries heat to the radiators at the same time. In service the oil oxidises slowly under oxygen and heat, and the acids and oxidation products formed stay dissolved at first, then, as they accumulate, become fine particles that drift and settle inside the tank. Acids react with metals in the tank to form metal soaps, adding to the sludge, and attack the cellulose paper insulation as well (USBR, 2003). Oil ageing shows mainly in interfacial tension and acidity: interfacial tension is the force needed to break the boundary between oil and water, and the acid number is the amount of potassium hydroxide that neutralises the acid in 1 g of oil (Elele et al., 2022).

So sludge is a result, and the cause lies in the conditions that oxidise the oil. Oxygen and heat drive oxidation, catalysts such as copper and moisture add to the ageing, and the oxidation inhibitor acts as a buffer that slows it. Oxidation is a chain reaction carried by free radicals, so conditions that make the reaction easier shorten how long the oil holds up (Zhang et al., 2024).

In such cases the technical team sets up the six hypotheses below and rules them out one by one. The start is always the same: gather several years of load and top-oil temperature records to see whether the temperature is rising at the same load, and set the interfacial tension, acid number, water content, dissolved oxygen and oxidation inhibitor content from the oil reports beside earlier values to read the trend.

Hypothesis 1: spent inhibitor

This hypothesis comes first when a transformer filled with inhibited oil has run for years without the inhibitor ever being measured or topped up. The same goes when routine analysis covers only dissolved gases, or when oil was added without checking whether it carried inhibitor. Think of a distribution transformer whose oil has not been touched since commissioning. The yearly reports list gas values in rows, the inhibitor line has been blank from the start, and a sample that was clear yellow a few years ago is visibly darker this year.

The oxidation inhibitor is a sacrificial substance that oxygen attacks instead of the paper. Like a sacrificial anode in cathodic protection it reacts with oxygen and is used up little by little, and once it is gone, oxygen attacks the cellulose insulation freely. The inhibitor used in transformer oil is mainly a phenolic compound called DBPC; the ideal content is 0.3% of the oil weight, oil at 0.08% is treated as uninhibited, and re-inhibiting is advised once it falls to 0.1% (USBR, 2000). The rate at which the inhibitor is used up can itself serve as a measure of oil life, and an accelerated ageing study measured oil life by the decline of the infrared absorption band that marks the inhibitor (Polanský et al., 2020).

The content can be measured straight from a sample. A standard method measures DBPC and its relative DBP by infrared absorption (ASTM International, 2021), so add this item when ordering routine oil analysis. One recommendation is to test it with the dissolved gas analysis once every 3 to 5 years (USBR, 2000). If the content is below the limit while the acid number rises year on year and interfacial tension falls, read it as oxidation proceeding without the inhibitor's protection. For a transformer being tested for the first time, check the oil type on the nameplate or commissioning papers to confirm that the oil was inhibited in the first place.

If the inhibitor is near the bottom, plan to re-inhibit. Set the amount from the nameplate oil weight and the gap to the target content, and expect that re-inhibiting usually requires treating the oil as well (USBR, 2003). Timing matters too. In accelerated ageing with copper, oil that received a second dose of DBPC, timed by changes in interfacial tension, saw its acidity rise 43.2% more slowly than oil with copper alone (Zhang et al., 2024). Match top-up oil to the same inhibited type, and log every addition and treatment in the oil records.

Hypothesis 2: oxygen and heat

Oxygen enters by the path the transformer breathes through. Each time the oil warms and cools its volume swells and shrinks, drawing air in and pushing it out; older open designs where air touches the oil directly, a torn rubber bag or diaphragm in the conservator, and damaged gaskets that let air leak in all belong here (USBR, 2000). Watch for this hypothesis most in transformers whose oil stays hot for long periods under summer load. Take a unit whose top oil climbs high every midsummer afternoon and stays there for hours, while the conservator bag has not been opened once in the twenty-plus years since it was fitted.

Oxygen dissolved in the oil reacts with hydrocarbon molecules to form free radicals, which attack further molecules in a continuing chain, and acids and polar products accumulate (Zhang et al., 2024). The reaction speeds up with heat, and a half-life rule, under which the oil's ageing rate doubles for every 7 °C rise in operating temperature, is used as the basis for accelerated ageing tests (Elele et al., 2022). Oxygen harms the paper as well. At the same temperature, cellulose insulation in low-oxygen oil lasts ten times longer than in high-oxygen oil, and one view holds that dissolved oxygen above 2,000 ppm greatly speeds paper deterioration (USBR, 2003).

In the dissolved gas report, look at oxygen and nitrogen together. When both are high it usually means a breach in the conservator bag or diaphragm, while under a nitrogen blanket high nitrogen with low oxygen is normal (USBR, 2003). Look at the colour of the breather silica gel, the oil level in the breather's oil cup and oil stains around gaskets and valves, and inspect the bag or diaphragm at the next outage. Compare samples taken from the same point by the same method, so that a rising yearly trend can be told from a single high reading.

Once the air path is found, close it first. Replace a torn bag or diaphragm, repair damaged gaskets, and swap discoloured silica gel for fresh. On older designs where air touches the oil, fitting a desiccant air dryer to the breather pipe is recommended (USBR, 2000). One guideline advises degassing the oil and adding fresh inhibitor once dissolved oxygen reaches 10,000 ppm (USBR, 2003). After the repair, confirm at the next analysis that oxygen in the same season has come down.

Hypothesis 3: copper catalysis

In a transformer with copper windings the oil is always in contact with copper, so the question is not whether copper is there but how far it has joined the reaction. Copper's effect grows when oil with an already raised acid number has been kept in service for long, when the oil runs hot, and when inhibitor is short. Say one unit, inhibited and with a sound breather, darkens its oil noticeably faster than others installed the same year. Opened at an outage, the paper around its windings shows a faint stain.

Copper acts as a catalyst, speeding oxidation without being consumed. In an experiment that aged oil and paper together, copper species attached to the paper fibre surface as nanoparticles and clustered, and the particle size grew from 27.06 nm to 94.19 nm as ageing progressed. The same study reports that monovalent and divalent copper act as active sites that set off free radical reactions, lowering the activation energy and making the oil easier to oxidise (Zhang et al., 2024). In another experiment that aged oil with a copper winding and kraft paper at 110 to 130 °C, these catalysts shortened oil life by 35 to 45% judged by colour change and by 35% judged by the inhibitor band (Polanský et al., 2020). Acids attack the metals in the tank to form soaps (USBR, 2003), so the higher the oil's acid number, the wider the way for copper to join the reaction.

Copper's share is hard to separate on the floor, so a laboratory comparison helps. The standard open-beaker method for ageing insulating oil has two procedures, with and without a metal catalyst (ASTM International, 2012), so the extent to which copper speeds oxidation of the same oil can be compared. On a transformer in service, track the acid number by the standard titration method (ASTM International, 2022) and read it alongside the inhibitor content. If the acid number climbs faster than on other units while inhibitor remains, suspect copper.

Copper cannot be removed from the windings, so the aim is to reduce the conditions it works under. Treat the oil before the acid number climbs, so there is less acid to dissolve copper, and keep the inhibitor at its target content. In the experiment above, the oil that was re-inhibited resisted copper-induced oxidation well (Zhang et al., 2024). Keeping the oil cooler points the same way, so check the cooling equipment as well.

Hypothesis 4: excess moisture

Water both gets in from outside and forms inside. It gets in when the breather silica gel is spent, when damaged gaskets on bushing heads or manhole covers let rain seep through, and when condensation forms on the inner tank walls of older designs where air touches the oil. In an old transformer, the paper itself gives off water as it ages. Picture a sample taken after the rainy season reading higher in water than last year, with water marks around a gasket on the tank top.

With water and oxygen together, the paper decays much faster and forms acids, metal soaps, sludge and more water. The acids formed speed the decay again, producing acid and water faster still, a vicious cycle. Most of the water in a transformer sits in the paper: the same water divides so that the paper holds 3,000 times as much as the oil at 20 °C and 300 times at 60 °C (USBR, 2003). Kraft paper gives off water as it ages, so its ageing accelerates itself, and acids are produced during ageing as well (Lundgaard et al., 2004).

Measure water from an oil sample, and always record the top-oil temperature at the time of sampling. Water moves between oil and paper with temperature, so the same ppm means different things at different temperatures; it is better read as moisture by dry weight of the paper or as percent saturation of the oil, not ppm alone. One guideline advises planning a dry-out when paper moisture reaches 2% by dry weight, and drying before it passes 2.5% or 30% oil saturation (USBR, 2003). Look over the breather, gaskets and bushing heads at the same time.

If water has indeed risen, close the leaks first and then dry. Repair damaged gaskets and bushing heads, change the silica gel, and fit a desiccant air dryer to older designs where air touches the oil. Moisture not only lowers the oil's insulating quality but also causes sludge to form (USBR, 2000). Most of the water sits in the paper, and drying the oil alone can let it come back out into the oil, so if moisture has passed the limit, plan a dry-out that reaches the paper with a specialist contractor.

Hypothesis 5: overloading

A plant that added equipment without adding transformer capacity, summer afternoons when cooling loads pile up, and a few stopped cooling fans that keep the unit from its rated cooling all have the same effect as overloading. A history of shifting load onto one transformer in an emergency belongs here too. One such case is a transformer that, since another production line was added, runs close to its nameplate rating every summer afternoon, with the winding temperature needle sitting well above where it used to.

As load rises, losses in windings and core turn into heat, and the top-oil temperature and the hot-spot temperature, the hottest point in the winding, rise together. The loading guide calculates the ageing rate of the insulation from the hot-spot temperature and treats time above the reference temperature as accelerated ageing (IEEE, 2011). Oil ageing likewise depends on loading and thermal stress (Elele et al., 2022). Sludge makes this worse. Sludge settled on the windings and structure lowers cooling efficiency, so the temperature creeps up at the same load (USBR, 2003), and the higher temperature speeds oxidation in turn.

Set the load records beside the temperature records. Compare hourly load with the nameplate rating, and see how top-oil and winding temperatures followed the load. Check whether any fan stands still on a hot, loaded day, and, with pumped cooling, whether pump current is normal. Sustained overloading generates combustible gases, and if the gas generation rate rises and falls with load, overloading can be suspected (USBR, 2000).

If overloading shows up, deal with load and cooling together. Repair failed fans and pumps, split load onto another transformer or add a cooling stage, and in the longer term plan for more capacity. When emergency loading is unavoidable, set the allowable time and temperatures in advance with the guide's calculation (IEEE, 2011). If sludge has already built up, the temperature will not return to its old level even with less load, so plan oil treatment and radiator cleaning alongside.

Hypothesis 6: products drop out

When a transformer whose oil has gone long without reclaiming or replacement shows a steady yearly rise in acid number and fall in interfacial tension, the oxidation products may already exceed what the oil can hold dissolved. This is the stage where the conditions above, accumulated over years, appear as visible sludge. A typical scene: a sample from the bottom valve left standing in a bottle settles a brown deposit, and the lower parts of a few radiator sections show up unusually cold.

Oxidation products are dissolved at first, but as they accumulate they become sludge particles suspended in the oil and then rain out inside the tank. The same products gather at the boundary between oil and water and weaken it, so interfacial tension falls. Clean new oil reads 40 to 50 dyne/cm, reclaiming is advised at 25 dyne/cm, and sludging begins around 22 dyne/cm. The same guideline notes that sludging begins when the acid number reaches 0.40 mg KOH/g and advises reclaiming at 0.20 mg KOH/g (USBR, 2003). This is why interfacial tension and acidity together serve as the main indicators of oil ageing (Elele et al., 2022).

Measure interfacial tension by the standard method that pulls a platinum ring up through the oil-water boundary (ASTM International, 2020), and follow it yearly together with the acid number. The direction of change matters more than any single value. Sediment and sludge in the oil can be measured separately by a method given in the oil maintenance guidance (IEC, 2013). If an infrared scan shows part of a radiator colder than the other sections, that section may be plugged with sludge or debris, so check the tubes by hand as well (USBR, 2000).

Once dropout has begun, filtering is not enough; the oil needs reclaiming that removes dissolved oxidation products and acids as well. Reclaiming is best done before interfacial tension and acidity reach the sludging values, so watch the trend and set budget and schedule ahead. If radiators are plugged with sludge, the transformer is probably sludged inside too, and one recommendation is to have a competent contractor reprocess the oil and clean the interior (USBR, 2000). After reclaiming, put the inhibitor back to its target content, or the same thing will happen again.

Finding the cause

The six hypotheses do not need to be investigated all at once. Rule out first what can be seen without an outage. Load and temperature records, fans and pumps, breather silica gel and oil stains around gaskets can all be checked in service. Next comes the analysis that one oil sample can settle, and work that needs an outage, such as inspecting the bag, cleaning radiators or internal inspection, comes last.

Oil analysis is the clue that carries the most information. Field and laboratory experience suggests that about 70% of the diagnostic information on a transformer's condition is held in the oil (N'cho et al., 2016). Pairs of results point the way. High oxygen with high nitrogen points to air leaking in, and high water with spent silica gel to water getting in. Low inhibitor with a rising acid number suggests spent inhibitor, while an acid number that climbs faster than on other units despite remaining inhibitor suggests copper catalysis. If interfacial tension and acidity are near the sludging values and parts of the radiator are cold, dropout has probably begun.

The shape of the temperature record is a clue too. If temperature rises and falls with load and is high only on summer afternoons, look first at overloading and the cooling equipment. If, at the same load, it has stepped up year by year, suspect sludge coating the cooling surfaces. When this does not settle it, run comparisons that change one thing at a time. Compare temperature at the same load after repairing the fans, and compare oxygen and water at the next analysis after fixing the breather. In the laboratory, the same oil can be aged with and without a metal catalyst to weigh copper's share.

The final check is the trend after the remedy. If the cause has been put right, the acid number should rise more slowly, the fall in interfacial tension should level off, and top-oil temperature at the same load should return to where it was. Check too that radiator sections that were cold on the infrared scan now match the others. If the figures do not recover, a cause is still left.

The hypotheses often overlap. Water and oxygen together set up a vicious cycle in which acid, sludge and water each make the others faster (USBR, 2003), copper triggers oxidation more easily when inhibitor is short, and settled sludge blocks cooling and raises the temperature, which speeds oxidation in turn. In such cases, close the paths for air and water first, reclaim the oil, re-inhibit it, and then match load and cooling. Change only the oil while the paths stay open, and the new oil goes the same way.

Limits and cautions

Control values for interfacial tension, acid number, water, dissolved oxygen and inhibitor differ by voltage class, transformer design, oil type and the guidance followed, so numeric decisions follow the oil specification, the oil maintenance guidance and the transformer maker's criteria. Judge by the trend of samples taken the same way, not by one result. If gases that point to an internal fault, such as acetylene, appear or gases rise quickly, get a specialist diagnosis first, separate from the sludge question.

Sampling from an energised transformer, adding inhibitor, reclaiming and drying oil and cleaning the interior are work for qualified staff and specialist contractors. Take care with nearby live parts, hot oil and pressure, and for the oil and any treatment chemicals follow the product's safety data sheet, the SDS, for protective equipment, ventilation and fire prevention. Dispose of drained oil and sludge as the relevant regulations require.

Sources

  1. ASTM International. (2012). ASTM D1934-95(2012), Standard test method for oxidative aging of electrical insulating petroleum oils by open-beaker method. https://store.astm.org/d1934-95r12.html
  2. ASTM International. (2020). ASTM D971-20, Standard test method for interfacial tension of insulating liquids against water by the ring method. https://store.astm.org/d0971-20.html
  3. ASTM International. (2021). ASTM D2668-07(2021), Standard test method for 2,6-di-tert-butyl-p-cresol and 2,6-di-tert-butyl phenol in electrical insulating oil by infrared absorption. https://store.astm.org/d2668-07r21.html
  4. ASTM International. (2022). ASTM D974-22, Standard test method for acid and base number by color-indicator titration. https://store.astm.org/d0974-22.html
  5. Elele, U., Nekahi, A., Arshad, A., & Fofana, I. (2022). Towards online ageing detection in transformer oil: A review. Sensors, 22(20), 7923. https://doi.org/10.3390/s22207923
  6. Institute of Electrical and Electronics Engineers [IEEE]. (2011). IEEE Std C57.91-2011, IEEE guide for loading mineral-oil-immersed transformers and step-voltage regulators. https://doi.org/10.1109/IEEESTD.2012.6166928
  7. International Electrotechnical Commission [IEC]. (2013). IEC 60422:2013, Mineral insulating oils in electrical equipment – Supervision and maintenance guidance. https://webstore.iec.ch/en/publication/2110
  8. Lundgaard, L. E., Hansen, W., Linhjell, D., & Painter, T. J. (2004). Aging of oil-impregnated paper in power transformers. IEEE Transactions on Power Delivery, 19(1), 230–239. https://doi.org/10.1109/TPWRD.2003.820175
  9. N'cho, J. S., Fofana, I., Hadjadj, Y., & Beroual, A. (2016). Review of physicochemical-based diagnostic techniques for assessing insulation condition in aged transformers. Energies, 9(5), 367. https://doi.org/10.3390/en9050367
  10. Polanský, R., Hahn, P., Kadlec, P., Moravcová, D., & Prosr, P. (2020). Quantifying the effect of catalysts on the lifetime of transformer oil. Applied Sciences, 10(4), 1309. https://doi.org/10.3390/app10041309
  11. U.S. Bureau of Reclamation [USBR]. (2000). Transformer maintenance (Facilities Instructions, Standards, and Techniques Vol. 3-30). U.S. Department of the Interior. Retrieved November 2026. https://www.usbr.gov/power/data/fist/fist3_30/fist3_30.pdf
  12. U.S. Bureau of Reclamation [USBR]. (2003). Transformer diagnostics (Facilities Instructions, Standards, and Techniques Vol. 3-31). U.S. Department of the Interior. Retrieved November 2026. https://www.usbr.gov/power/data/fist/fist3_31/fist3-31.pdf
  13. Zhang, H., Zhang, Z., Yan, J., Wang, S., Huang, X., Zuo, F., Li, A., Gao, F., Lin, H., & Wang, B. (2024). Revealing the intrinsic correlation between Cu scales and free radical chain reactions in the regulation of catalytic behaviour. Molecules, 29(19), 4690. https://doi.org/10.3390/molecules29194690

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.