Switching to a different film is the usual response when parts rust in VCI packaging, but VCI works only when its vapour fills an enclosed space and stays there, so once that condition breaks, rust tends to return even with another film. What actually lies behind it can be poor seals and openings, moisture and contamination left on parts before packing, too little time for the vapour to build up, surfaces the vapour cannot reach, or film whose inhibitor is spent, and sometimes two or more at once.

Background

A customer opens a crate that has spent weeks at sea and finds red rust spots spreading over gears and shafts inside VCI film bags. The rust is uneven from part to part; one crate is fine, while in another it is concentrated on the parts in one corner. Rework to strip the rust and re-protect, scrap where precision faces cannot be recovered, customer claims and reshipment follow, and every shipment already sent in the same packing becomes a worry.

A volatile corrosion inhibitor, VCI, is a substance that evaporates from film or paper, spreads through the air of an enclosed space, and condenses and adsorbs on the metal surfaces inside, slowing corrosion (NACE International, 2008). Rust, for its part, needs a water layer on the steel surface, and that layer forms more readily the higher the relative humidity and when salt or dust is on the surface (Leygraf et al., 2016). So VCI does not remove water; it works by filling the space with enough vapour to build an adsorbed film on the surface and holding off attack by water while that film lasts. How the vapour reaches the surface, how its vapour pressure changes with temperature, and the conditions under which the adsorbed film forms and breaks down decide the effect (Bastidas et al., 2005).

So rust inside VCI packing raises two questions: whether vapour built up enough at that part's surface and stayed, and whether water and contamination went beyond what the film could withstand. With the same film, the answers change with how the parts were wrapped, their condition before wrapping and the conditions after sealing.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: photograph the packs before opening them, record on which faces of the parts and where in the pack the rust formed, then compare the packing date and conditions and the film's production lot with the film's technical data sheet, the TDS.

Hypothesis 1: leaking seal

This hypothesis comes to the front when the closure of the pack is not intact. That means bag mouths folded over rather than heat-sealed or taped only in places, film torn by sharp edges or forklift tines, packs opened for inspection and not closed again, and crate liners left open at a corner. Here is one crate: a VCI liner was laid in a wooden export crate and filled with parts, and in the rush one corner was only folded over before the lid went on. On arrival, rust spots have spread from the parts nearest that corner, while the parts on the far side are clean.

What VCI protects is a space. The amount needed is set by the enclosed volume rather than the weight of the parts, and gaps, loose wrapping and open seams lower the vapour concentration inside (ZERUST, n.d.-b). Poor seals or frequent opening delay the build-up of vapour and weaken protection (ZERUST, n.d.-a). Through an opening, vapour escapes while humid outside air moves in and out, so rust tends to start on the parts nearest the opening. The military specification for VCI-treated transparent film likewise defines it as a heat-sealable barrier material (DoD, 2006).

Photograph before tearing anything open. Shoot each seal line, tape joint, corner and tear, number the positions of the parts in the crate, and map the distance between rusted parts and openings. If rust starts close to an opening and fades with distance, this hypothesis is strong. Check the shipping documents too for any record of the packs being opened for inspection or customs.

Make sealing a process step. Heat-seal bag mouths all the way across, and when closing with tape, wrap it over the whole joint. Pad sharp edges so the film does not tear, and add a seal check to the packing checklist, together with a rule that any pack opened for inspection is resealed on the spot.

Hypothesis 2: wet or dirty parts

The starting point for this hypothesis is a line that wraps parts the moment washing or machining ends. It covers parts wrapped before water-based cleaner or coolant has dried, parts wrapped still warm from the washer, parts brought in from outside on a rainy day, and parts handled with bare hands. Shafts came out of an aqueous washer still warm, went into VCI bags and were sealed at once; the next day droplets had formed on the inside of the bags. Opened a few weeks later, the shafts show rust along their undersides where the droplets collected and in the shape of fingerprints.

Rust needs water. The water layer on steel thickens as relative humidity rises, and contamination that attracts water, such as salt left by sweat or cleaner, lets water form at lower humidity, so corrosion starts there (Leygraf et al., 2016). The adsorbed film VCI builds forms and breaks down depending on surface pH and water, so when there is enough water to pool, the film struggles to hold (Bastidas et al., 2005). When warm parts are sealed in, vapour in the pack's air condenses on the cool inside of the film or on the parts as they cool. That is why manufacturers advise letting parts cool before sealing and not trapping standing water or excess moisture (ZERUST, n.d.-a).

The pattern of the rust tells the story. Fingerprint shapes point to bare-hand handling, outlines like the edge of pooled water on the underside point to condensed or leftover water, and tracks where cleaner ran point to cleaning residue. Find the part temperature and workshop relative humidity at packing time in the records, and if there are none, measure them at the next packing. Wipe part surfaces just before packing with a clean cloth, rinse the cloth in water and measure the conductivity; that puts leftover salt in numbers for comparison.

Set standards for the state of parts before wrapping. Wrap parts only when fully dry and cooled to room temperature, and after aqueous washing rinse off leftover cleaner and dry. Wear gloves for packing work, and dry parts wet by rain before handling them further. Keep the packing area in a dry spot away from outside doors, and add boxes for part temperature and humidity at packing to the checklist.

Hypothesis 3: vapour not built up

This hypothesis covers goods moved into a cold container or truck within hours of sealing, packing done in winter where there is no heating, and large volumes given only a little VCI material. Suppose crates sealed late in the afternoon were loaded into a container that same night and sent to the port. Overnight the temperature fell sharply and droplets formed inside the container, and on arrival the crates sealed last have more rust than those sealed first.

VCI does not act at once. Vapour from the film has to fill the space and adsorb on the metal to form a film, and this adsorption, with the protective after-effect that remains, is the core of the inhibition (Andreev & Kuznetsov, 2005). Vapour pressure changes with temperature, so vapour builds up more slowly in the cold (Bastidas et al., 2005). The standard test of the vapour-inhibiting ability of VCI materials places the sample and a steel specimen in a small sealed jar and leaves it for 20 hours to let the vapour build up before the specimen is chilled to make water condense (NACE International, 2008). Send a large crate into condensing conditions straight after sealing, and water can arrive before the vapour has built up.

The check is to line up the timeline. Match each crate's sealing time, dispatch and loading times, and temperature changes in transit from the documents and a temperature and humidity logger, and compare rust in crates that left straight after sealing with crates that stayed a few days. If the later a crate was sealed, the more it rusted, this hypothesis gains weight. If the film's TDS gives a time for protection to establish or an amount per volume, compare those with the actual packing.

Build a waiting time after sealing into the process. Hold sealed packs somewhere with steady temperature for the time the supplier recommends before dispatch, and heat the packing area in winter. For large volumes, work out with the supplier an amount of VCI matched to the volume so the film alone is not left short. If shipping schedules are tight, move packing earlier rather than shorten the wait.

Hypothesis 4: vapour cannot reach

Weigh this hypothesis when only the inside of a large crate is lined with VCI film and the parts within are wrapped again in ordinary plastic bags or cardboard boxes, and for parts with deep bores and blind holes, hollow castings, or several parts nested together. Lift a gear housing out of a lined crate: the outer faces that faced the liner are clean, but rust has filled only the inner bore and the blind tapped holes.

Vapour protects only where it reaches as it spreads through the air. VCIs are compounds that evaporate, spread through the space and adsorb on metal surfaces, and substances that work this way are used for both ferrous and non-ferrous metals (Subramanian et al., 2000). When the path is long or blocked, too little vapour reaches the surface. Manufacturer guidance, too, treats cavities, blind holes and overlapping surfaces as blocking vapour movement and creating dead-air pockets, and recommends adding vapour-emitting devices inside such parts (ZERUST, n.d.-b). If ordinary plastic film sits between the VCI film and the part, vapour cannot pass through it, so the part is in effect inside a bag with no VCI.

See what lay between the rusted face and the VCI material. Distinguish rust only in shielded places such as bores, blind holes and inside nested faces from rust on outer faces too. Confirm from labels and supply records whether the inner packaging was VCI-treated or ordinary material, and measure the distance from the VCI film to the rusted spot against the conditions of use in the TDS. Comparing parts in the same crate that sat right against the VCI with parts that sat apart makes the difference plain.

Bring the VCI closer to the parts. Rather than relying on one big liner, wrap each part in a VCI bag or paper, and switch the inner packaging to VCI-treated material too. Put vapour-emitting devices inside deep bores and hollow castings, or fit VCI plugs into the holes. Separate parts that were nested with VCI paper between them.

Hypothesis 5: spent film

The subjects of this hypothesis are film rolls that have spent a long time in a corner of the warehouse, rolls opened and left part-used, rolls kept in sunlight or heat, and bags reused after one trip. It is the case where only the parts wrapped from a half-used roll that sat on a windowsill shelf for months rust, while parts wrapped the same day from a freshly opened roll stay clean. The two rolls look no different.

The VCI in film escapes little by little. One manufacturer gives a shelf life of up to three years in the original airtight packaging, yet states that exposure to heat, UV or open air reduces effectiveness, that shelf life can shorten once the packaging is opened, and that the film may look unchanged while the inhibitor concentration is already too low (ZERUST, n.d.-c). Vapour pressure rises with temperature, so the warmer a roll is kept, the faster inhibitor leaves it (Bastidas et al., 2005). A reused bag has already given off inhibitor during its first use, and vapour can leak through creases and scuffs.

Start with the roll's production date and storage history. Compare the lot and date on the roll label with the shelf life in the TDS, and find out where the roll was kept and how long it lay open. Match the packing records to see whether rust clusters in packs wrapped from one roll or lot. Comparing a suspect roll with a fresh one in the standard vapour-inhibiting ability test, or in a side-by-side coupon trial under the same conditions, shows whether inhibitor remains (NACE International, 2008).

Manage film like any stock. Use it in the order received, reseal part-used rolls and keep them somewhere cool and shaded. Mark opening dates on rolls and bags, and do not use stock past its shelf life until a test has confirmed it. Make it a rule not to reuse bags.

Finding the cause

Work through the five hypotheses starting with what is easiest to check. The state of the packs and where and how the rust formed can be seen the day the crate is opened, and packing times, shipping schedules and film lots are in the documents. Film tests and coupon comparisons take days to weeks, so they come next.

The biggest clue is where the rust is. More rust nearer an opening points to poor seals and openings, and rust only in shielded places such as bores and blind holes points to vapour that could not reach. Rust following fingerprints or the edge of pooled water points to moisture and contamination left before packing. Rust clustered in packs wrapped from one roll, regardless of crate or position, points to spent film.

Next comes time. More rust in crates sealed late and sent off at once means the vapour had too little time to build up, while droplets inside the bags within days of packing mean the parts were wrapped wet. If rust rises and falls with the season under the same film and packing method, look at condensing conditions and build-up time together.

If that still does not settle it, run control trials. Split parts from one lot and change the packing for one group only, choosing one of heat sealing, packing after full drying and cooling, a day's wait after sealing, wrapping each part in VCI, or a fresh roll, and send both groups by the same route with a temperature and humidity logger inside. Change only one thing at a time, or there is no telling which one worked. Afterwards, count rusted parts per crate on the same basis, and the job is done only when that figure has recovered.

The hypotheses can overlap. An open gap lets vapour out and humid air in, wet parts add to that moisture, and if condensation arrives before the vapour has built up, spent film holds out less well. In such cases deal with water first. Make sure dry, cooled parts go into packs sealed all the way round, then look at waiting time, VCI placement and film condition, because while water keeps getting in, the effect of changing anything else cannot be compared fairly.

Limits and cautions

The amount of VCI, the time for protection to establish, shelf life and the metals a product suits differ by product, so numeric decisions follow the film's TDS and the supplier's guidance. VCI cannot remove rust that has already formed, so strip rust from parts before packing. If wooden crates are used, keep under-dried timber out of the pack itself, because even very small amounts of acetic acid vapour from wood increase corrosion of steel when humidity is high (Clarke & Longhurst, 1961). Where copper or other non-ferrous metals go into a pack with steel, confirm that the product suits those metals as well; the standard test includes a separate, optional check that VCI-treated material does not corrode copper (NACE International, 2008). For parts where a single rust spot rules out use, such as precision bearing faces or aerospace parts, do not return them to service on floor judgement alone; get the quality engineer's judgement.

Safety matters too. Handle VCI materials, cleaners and preventives according to the product's safety data sheet, the SDS, and when opening large liners or containers, ventilate the air inside for a while before starting work. Use heat sealers with care to avoid burns, and wear eye protection and gloves when removing rust. Follow lifting procedures when taking out and repacking heavy parts.

Sources

  1. Andreev, N. N., & Kuznetsov, Y. I. (2005). Physicochemical aspects of the action of volatile metal corrosion inhibitors. Russian Chemical Reviews, 74(8), 685–695. https://doi.org/10.1070/RC2005v074n08ABEH001162
  2. Bastidas, D. M., Cano, E., & Mora, E. M. (2005). Volatile corrosion inhibitors: A review. Anti-Corrosion Methods and Materials, 52(2), 71–77. https://doi.org/10.1108/00035590510584771
  3. Clarke, S. G., & Longhurst, E. E. (1961). The corrosion of metals by acid vapours from wood. Journal of Applied Chemistry, 11(11), 435–443.
  4. Leygraf, C., Odnevall Wallinder, I., Tidblad, J., & Graedel, T. (2016). Atmospheric corrosion (2nd ed.). Wiley.
  5. NACE International. (2008). NACE TM0208-2008, Laboratory test to evaluate the vapor-inhibiting ability of volatile corrosion inhibitor materials for temporary protection of ferrous metal surfaces.
  6. Subramanian, A., Natesan, M., Muralidharan, V. S., Balakrishnan, K., & Vasudevan, T. (2000). An overview: Vapor phase corrosion inhibitors. Corrosion, 56(2), 144–155.
  7. U.S. Department of Defense [DoD]. (2006). MIL-PRF-22019E, Barrier materials, transparent, flexible, heat-sealable, volatile corrosion inhibitor treated.
  8. ZERUST. (n.d.-a). How long does it take for VCI to work inside a sealed package? Manufacturer guidance. Retrieved November 2026. https://www.zerust.com/?p=7176
  9. ZERUST. (n.d.-b). How much VCI must be placed in the packaging? Manufacturer guidance. Retrieved November 2026. https://www.zerust.com/faq/how-much-vci-must-be-placed-in-the-packaging/
  10. ZERUST. (n.d.-c). What is the shelf life of VCI film? Manufacturer guidance. Retrieved November 2026. https://www.zerust.com/faq/what-is-the-shelf-life-of-vci-film/

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.