KALTECKOREA

BlogApplication notes

Why do copper and zinc parts tarnish in VCI packaging?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Corrosion Prevention

When copper or zinc parts tarnish inside VCI packaging, the usual response is to assume there was too little inhibitor and add more, but some VCIs made for steel fail to protect non-ferrous metals or even attack them, so more of the same does not solve it. What actually lies behind the tarnish can be steel-only VCI chemistry, several metals packed together, damp inside the pack, sulphur in the packaging or temperature swings, and sometimes two or more at once.

Background

A customer opens a VCI bag to find the steel parts clean, while the brass fittings packed with them are stained brown or black and the zinc-plated brackets carry a white powder. Discolouration has appeared inside packaging meant to stop corrosion, so the customer distrusts the whole pack. Parts where appearance matters come back, the remaining stock has to be opened and cleaned or replated, and parts headed for soldering or painting need their surfaces prepared again.

A VCI, a volatile corrosion inhibitor, evaporates from the packaging, spreads through the air of a closed space, then condenses and adsorbs on metal surfaces or dissolves into the thin water film on them, slowing corrosion (NACE, 2008). How well an inhibitor protects a metal depends on how its molecules attach to that particular metal surface, and the molecular structure sets that behaviour (Andreev & Kuznetsov, 2005). So an inhibitor that works well on one metal is no guarantee of the same effect on another.

Copper and zinc also change in air differently from steel. Atmospheric corrosion happens inside a thin water film on the metal, and gases from the air dissolve into that film and drive the reaction. Copper darkens from an oxide towards products such as sulphides, while zinc forms white products such as hydroxides and carbonates (Leygraf et al., 2016). Tarnish is a very thin layer of these products, so finding what made the water film and what dissolved into it points to the cause.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: check which metals the VCI material's technical data sheet, the TDS, says it is for, record the parts' condition and humidity at packing, the other materials in the pack and the shipping and storage route, and match these against where in the pack the tarnished and the clean parts sat.

Hypothesis 1: steel-only VCI

This hypothesis comes up first where a plant has standardised on one packaging material and uses VCI paper or film bought for steel parts on copper, brass and zinc parts as well. It also applies when new non-ferrous parts come in, when the packaging supplier changes, or when the purchase specification does not say which metals the material is for. Say a store still holds plenty of VCI bags bought for steel parts, so the same bags go on a new order of brass connectors. A few weeks later the customer opens a bag to find the connectors evenly darkened, while the steel parts in the same bags draw no complaints.

Volatile inhibitors were first developed to protect steel, and it was recognised early that many of the inhibitors used for steel were incompatible with non-ferrous metals (Subramanian et al., 2000). In a study of dicyclohexylamine nitrite, a widely used inhibitor, it slowed corrosion of mild steel by blocking the anodic reaction, but on zinc it bonded to the surface, formed a soluble complex and sped corrosion up instead (Khamis et al., 2001). Copper is typically protected by azole inhibitors such as benzotriazole, which build a complex film on its surface, so a steel formula without such components struggles to protect copper (Finšgar & Milošev, 2010).

A material that has passed the standard test does not rule this out. The standard test of a VCI's vapour-inhibiting ability is judged on steel specimens only, the check for whether the material corrodes copper is optional and done only when the manufacturer or user asks for it, and other non-ferrous tests are outside its scope (NACE, 2008). So first see whether the TDS and test report list copper and zinc as covered metals and whether a copper compatibility check was done. On the floor, seal freshly cleaned copper and zinc strips in a jar with the suspect material, keep an identical jar without the material beside it, and compare the colours later; any difference shows up.

If the material proves unsuitable, switch to a non-ferrous product or a multi-metal product made to protect several metals together, and ask the supplier for compatibility test results on copper and zinc. In the store, keep steel and non-ferrous materials apart, label them clearly by metal so they are not mixed up, and write the covered metals into the purchase specification as well.

Hypothesis 2: metals packed together

Consider this hypothesis when one assembly mixes metals, such as a valve with a steel body, brass nipples and zinc-plated bolts, or when several parts go out together in one box as a kit. The same holds when parts of different metals are stacked in one bag to save space. Picture a batch of finished valves sent abroad in one bag: on arrival the steel bodies are sound, but white corrosion product has gathered on the heads of the zinc-plated bolts, mostly around the spots where they touch the brass nipples.

Mixing metals sets two things going at once. One is galvanic corrosion. When two different metals touch with a water film between them, they form a cell and the more active one corrodes faster. Which one corrodes is estimated from the galvanic series, the order of corrosion potentials measured in the same environment, and the further apart the two metals sit in that series, the greater the driving force tends to be (ASTM International, 2021). Zinc is more active than steel and copper, so it is sacrificed first in such pairs.

The other is a clash over inhibitor amount and type. In tests on zinc coupled to steel, the inhibitor's effectiveness depended mainly on its concentration (Khamis et al., 2001). In research on amine inhibitors, the amount of amine that fully stopped zinc corrosion was smaller than that needed for steel, and a vapour made of amines alone could push the surface pH above 10, too high to protect zinc (Valente et al., 2017). An inhibitor dosed generously for steel may therefore be too much for zinc. Start checking by seeing whether the tarnish gathers where a part touches another metal or right around that spot. Product spreading out from the contact points suggests a galvanic pair, while zinc parts damaged evenly all over the pack point back to the inhibitor.

If a galvanic pair is to blame, put dividers or VCI paper between the metals so they do not touch, and pack each metal separately where possible. For assemblies that cannot be split, list every metal they contain, choose a multi-metal product, and get the supplier's test data for that combination. Keeping water films from forming inside the pack matters here too.

Hypothesis 3: damp inside the pack

A pack becomes damp when parts washed in water-based cleaner or cutting fluid are packed before they are dry, when packing is done on a humid day with the shop doors open, when wet cardboard or wooden pallets are used, or when a torn bag lets outside air in. Take an afternoon in the rainy season when parts still warm from the washer go straight into a bag and the mouth is folded shut. A few weeks later the faces where zinc parts touch are thick with white powder, and the copper parts carry stains shaped like water drops.

Water speeds atmospheric corrosion because the reaction runs inside the surface water film. The thicker the film and the longer it stays, the more gas and salt dissolve into it and keep the reaction going (Leygraf et al., 2016). On zinc this shows as wet storage stain, often called white rust. A drop trapped between stacked parts gets less oxygen at its centre than at its edge, so it becomes a cell in which the centre dissolves and the edge takes up oxygen and carries the other half of the reaction, and zinc oxide and zinc hydroxide build up as a white powder. The product takes up three to five times the volume of the zinc it came from, so the attack looks worse than it is, and chlorides or sulphur compounds in the water make it faster (AGA, 2014). Copper also sulphidises within the same kind of film, and in experiments humidity strongly controlled the rate of copper sulphidation (Graedel et al., 1985).

The shape of the stain is the first clue. White powder or drop marks gathered on faces where parts touch, at the bottom of the bag, or wherever water can pool are signs of trapped water. Feel the parts just before packing for damp or cleaner residue, and put a humidity indicator card or a small temperature and humidity logger in a bag of the next shipment to record conditions inside the pack. Measure the moisture content of cardboard and wooden pallets with a moisture meter.

Once damp is identified, build full drying and cooling to room temperature into the process before packing. Pack in a low-humidity area, use only dry packaging materials and seal bags without holes. For long storage or humid routes, review adding desiccant with the packaging supplier, and space zinc parts so they do not stack and trap water.

Hypothesis 4: sulphur in packaging

Suspect sulphur in packs where parts are bundled with rubber bands, packed with rubber pads or cushioning, or wrapped in wool felt. The same goes for assemblies with rubber seals inside. Sometimes a bundle of brass parts is tied with a rubber band and bagged. When the bag is opened, the rest of each part is fine, but a black band runs where the rubber was wrapped, and the parts nearest the band are the darkest.

Sulphur-crosslinked rubber and protein materials such as wool are known to release sulphur compounds inside closed spaces, and hydrogen sulphide among them tarnishes silver and copper within a very short time. High humidity, above roughly 70% relative humidity, starts and speeds corrosion (Tétreault, 2021). An experimental study that sulphidised copper and silver with hydrogen sulphide proposed that the sulphur gas first dissolves in the surface water film and the dissolved gas then bonds directly with metal atoms to form sulphide (Graedel et al., 1985). A sealed bag is not diluted by outside air, so gas released by the packaging stays inside and keeps meeting the copper surface.

If the tarnish is dark where rubber or felt touched, or close by, and fades with distance, this hypothesis gains weight. Suspect materials can be screened with the accelerated corrosion test that museums use to choose storage materials. Silver, copper and lead coupons are sealed with the test material at raised temperature and humidity and then compared with a control vessel without it; silver responds to sulphur-type gases (Robinet & Thickett, 2003). Without a laboratory, sealing a suspect material with a freshly cleaned copper strip and comparing it with a control jar still gives a lead.

When only the strip sealed with the rubber or felt has darkened, take rubber bands, rubber cushioning and wool felt out of the pack and replace them with materials tested not to give off sulphur. Where a rubber part cannot be removed, as in an assembly, wrap it so it does not touch copper parts, and keep the humidity in the pack low to reduce the water film the gas can dissolve into. Recheck the new materials with the same sealed test.

Hypothesis 5: temperature swings

Temperature changes make things worse on long voyages in shipping containers, in unheated warehouses or under outdoor shelters, in seasons with large day-night swings, and when packs brought in from the cold are opened straight away in a warm room. A box of copper parts shipped by container in summer spends weeks heating up by day and cooling by night. On arrival, the inside of the bag shows dried drop marks, and parts in the upper boxes carry more stains.

Warm air holds more water, and when a metal surface in contact with it cools below the dew point, water condenses. As air inside a pack warmed by day cools at night, dew settles on the cold metal, and each repeat of this wetting and drying lays down a fresh water film (Leygraf et al., 2016). The inhibitor changes too. A VCI's vapour pressure varies with temperature, so in heat the inhibitor comes off faster, and if the bag is not well closed it escapes faster as well, which can shorten the protection period (Bastidas et al., 2005). The standard test, too, checks inhibiting ability in warm, water-saturated air followed by condensing water, and judges the result on steel specimens (NACE, 2008).

This hypothesis cannot be settled without knowing the temperature and humidity in transit and storage, so put a logger in the next shipment to record the highest and lowest temperatures, the humidity and the time spent at the dew point. See whether stains gather in upper or outer boxes or on the sunny side, and whether the inside of the bag shows drop marks. If the same pack stays fine in an indoor store and tarnishes only after a long journey, lean towards temperature.

When the logger shows long spells at the dew point, add an insulating layer outside the pack or use container desiccants, and stack boxes away from sunlight and the container walls. Leave packs brought in from the cold closed until they reach room temperature, then open them. Give the packaging supplier the transit time and temperature range and confirm the product's protection period suits those conditions.

Finding the cause

There is no need to investigate all five hypotheses at once. Rule them out starting with what can be checked on paper or by eye. The material's covered metals and test report can be read at a desk, and whether rubber or felt is in the pack or different metals touch is plain once the bag is open. Humidity and temperature need a logger and one shipment to watch, so they come next.

The shape and place of the tarnish are the best clues. If parts of the same metal changed evenly throughout a pack regardless of position, look first at the inhibitor chemistry of the packaging. Tarnish gathered where parts touch another metal points to a galvanic pair; white powder or drop marks on stacked faces and at the bottom of the bag point to trapped water; a black band where rubber or felt touched points to sulphur; and stains only in upper boxes, on the sunny side or after long journeys point to temperature swings. Copper turning black leans towards sulphides, while white powder on zinc leans towards water and the inhibitor.

If that still does not settle it, run sealed-jar control trials. Put freshly cleaned copper and zinc strips into several jars: one with only the VCI material in use, one with only the rubber band or felt, and one with nothing added, all kept in the same place. Change only one thing per jar, or there is no telling what caused the tarnish. To see the effect of humidity, repeat the same set-up with dry strips and with lightly wetted strips.

The final check is real shipments. Send the next few shipments in the revised packaging with loggers, open the bags on arrival and record any tarnish on the same basis as before. The job is done only when the tarnish has gone and the logger's humidity and dew point records have settled too.

The hypotheses often overlap. Damp and temperature swings create the water film, and that film is what lets sulphur gas dissolve, a galvanic cell run and amines raise the pH of a zinc surface. So when several causes appear together, first dry the inside of the pack and reduce the temperature swings, then go back over the packaging chemistry, the metal combination and any sulphur-bearing materials in turn. While a water film remains, the effect of changing anything else is hard to compare fairly.

Limits and cautions

Covered metals, protection period, amount of material and sealing conditions differ by VCI product, so figures and directions follow the product's TDS and the supplier's test data. For parts mixed with other non-ferrous metals such as silver, tin, lead or magnesium, and for products whose function depends on the surface, such as electronic or optical parts, do not settle the packaging on floor judgement alone; test compatibility on the actual metals with the supplier. Cleaning, replating and whether tarnished parts can be used follow the quality engineer and the customer specification.

Safety matters too. Handle VCI packaging, inhibitor powders and tablets according to the product's safety data sheet, the SDS, keep powders from becoming airborne, and wear protective equipment. For acidic cleaners used to remove tarnish, follow the SDS for protective equipment and ventilation, and ventilate large packs or containers that have been sealed for a long time after opening them, before going in.

Sources

  1. American Galvanizers Association [AGA]. (2014). A guide to minimizing and treating wet storage stain on hot-dip galvanized steel. https://galvanizeit.org/uploads/publications/Wet_Storage_Stain_On_Galvanized_Steel.pdf
  2. Andreev, N. N., & Kuznetsov, Yu. I. (2005). Physicochemical aspects of the action of volatile metal corrosion inhibitors. Russian Chemical Reviews, 74(8), 685–695. https://doi.org/10.1070/RC2005v074n08ABEH001162
  3. ASTM International. (2021). ASTM G82-98(2021)e1, Standard guide for development and use of a galvanic series for predicting galvanic corrosion performance. https://store.astm.org/g0082-98r21e01.html
  4. Bastidas, D. M., Cano, E., & Mora, E. M. (2005). Volatile corrosion inhibitors: A review. Anti-Corrosion Methods and Materials, 52(2), 71–77. https://doi.org/10.1108/00035590510584771
  5. Finšgar, M., & Milošev, I. (2010). Inhibition of copper corrosion by 1,2,3-benzotriazole: A review. Corrosion Science, 52(9), 2737–2749. https://doi.org/10.1016/j.corsci.2010.05.002
  6. Graedel, T. E., Franey, J. P., Gualtieri, G. J., Kammlott, G. W., & Malm, D. L. (1985). On the mechanism of silver and copper sulfidation by atmospheric H2S and OCS. Corrosion Science, 25(12), 1163–1180. https://doi.org/10.1016/0010-938X(85)90060-5
  7. Khamis, E., Oun, S. R., & Lyon, S. B. (2001). Use of dicyclohexylamine nitrite in inhibition of coupled zinc and steel. British Corrosion Journal, 36(3), 197–200. https://doi.org/10.1179/000705901322914070
  8. Leygraf, C., Odnevall Wallinder, I., Tidblad, J., & Graedel, T. (2016). Atmospheric corrosion (2nd ed.). Wiley.
  9. NACE International. (2008). NACE Standard TM0208-2008, Laboratory test to evaluate the vapor-inhibiting ability of volatile corrosion inhibitor materials for temporary protection of ferrous metal surfaces. NACE International.
  10. Robinet, L., & Thickett, D. (2003). A new methodology for accelerated corrosion testing. Studies in Conservation, 48(4), 263–268. https://doi.org/10.1179/sic.2003.48.4.263
  11. Subramanian, A., Natesan, M., Muralidharan, V. S., Balakrishnan, K., & Vasudevan, T. (2000). An overview: Vapor phase corrosion inhibitors. Corrosion, 56(2), 144–155. https://doi.org/10.5006/1.3280530
  12. Tétreault, J. (2021). Agent of deterioration: Pollutants. Canadian Conservation Institute. Retrieved November 2026. https://www.canada.ca/en/conservation-institute/services/agents-deterioration/pollutants.html
  13. Valente, M. A. G., Jr., Teixeira, D. A., Azevedo, D. L., Feliciano, G. T., Benedetti, A. V., & Fugivara, C. S. (2017). Caprylate salts based on amines as volatile corrosion inhibitors for metallic zinc: Theoretical and experimental studies. Frontiers in Chemistry, 5, 32. https://doi.org/10.3389/fchem.2017.00032

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.