KALTECKOREA

BlogApplication notes

Why does wire keep breaking during drawing?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Metalworking Fluids (MWF)

Blaming the rod or slowing the line is the usual response to wire breaking during drawing, but wire breaks when the pull exceeds what it can bear at that point, so unless the condition that raised the pull or weakened the wire is found, breaks tend to return. What actually lies behind them can be a thin lubricant film, a worn or wrong die, faulty pretreatment, overheated lubricant or a flawed rod, and sometimes two or more at once.

Background

A drawing machine running at speed stops dead, with a broken wire end caught between dies. Each break means pointing the end again and rethreading die by die, so the line stands, and wire on either side of the break is scrapped as short lengths or moves on to the next process with a joint in it. The finer the stage at which it breaks, the more processing is thrown away with it, and a whipping wire end can injure someone.

Drawing pulls wire through a die hole smaller than the wire itself to make it thinner. The pull has to be carried by the thinner wire that has just left the die, so when the drawing stress on the wire at the die exit exceeds that wire's strength, the wire breaks. Drawing stress is made up of the work to reduce the diameter, friction between die and wire, and redundant work, the extra deformation forced by the die angle; the die angle and the reduction, the share of cross-section removed in one pass, together set the size of each (Wright, 2016).

So a wire breaks in one of two ways: the pull rises because friction or redundant work grows, or the wire is weakened locally by a flaw or by embrittlement. Lubricant, die, pretreatment, heat and the rod itself all lead into one of these two, so where the wire broke and what the break looks like narrow the cause sharply.

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: keep both broken ends, log at which die and when the break happened, with the speed and lubricant condition at the time, and compare them with the lubricant's technical data sheet, the TDS, and the machine settings.

Hypothesis 1: thin lubricant film

When breaks increase in dry drawing, where soap powder fills a box in front of each die, that die box is the first place to look. It happens especially when the powder runs low and the wire no longer passes through it, when damp powder cakes into lumps, when only the powder around the wire is pushed aside and leaves an empty channel, and when the speed has gone up but the soap grade has not. Picture a die box near the end of a shift. Powder remains at the edges, but the path of the wire has been hollowed out, and the wire enters the die with almost no powder on it. Breaks that did not happen early in the shift now appear at the later dies.

The soap's job is to build a thin film between die and wire. The wire drags soap into the die entry, and in the narrowing gap the soap is pressed and heated until it flows and keeps die and wire apart. In tests on stainless steel wire, a mixture of the salt coating on the wire and the soap gave lubrication close to a fluid film, with calcium stearate soap suited to low speeds and sodium stearate soap to high speeds (Felder et al., 2011). In a model study, the thickness of the film dragged in varied with how the soap flows when heated and with several process conditions (Montmitonnet et al., 1982). When the film thins or breaks, die and wire touch directly and the friction coefficient rises; in simulations, die surface temperature and die wear rose along with it (Suliga et al., 2025). Drawing stress climbs with the friction, and once it reaches the wire's strength, the wire breaks (Wright, 2016).

Look inside the die box first. Check the powder level, any empty channel around the wire, lumps and damp, and if the box has a stirrer, check that it turns. Then cut a short sample of wire after each die and look at the surface. See whether the film covers it evenly, and read scratch lines or bare metallic shine as signs that the film broke at that die. The lubricant left on the wire can be compared die by die in numbers by weighing a set length of wire before and after cleaning, the same residual film weight measured in laboratory studies (Felder et al., 2011).

If the film shows signs of thinning, restore the soap's path to the wire first. Top up the die box before it falls below a set level, and use a stirrer or a rotating box so no channel forms. Store powder sealed and dry, and scoop out caked or long-used powder. If the speed has changed, choose a soap grade for that speed with the supplier again. Whether the wire carries enough coating to hold the soap is checked along with pretreatment.

Hypothesis 2: worn or wrong die

If breaks always happen at the same die position, suspect the die. Typical cases are dies run past their change interval, dies whose angle or bearing length changed in regrinding, die sets mixed with dies from another line after a size change, and the period right after a new reduction schedule. Think of the week of a size change, when a few dies were brought over from another line. Lubricant and rod are unchanged, yet the wire breaks near the same die every time, and the wire leaving that die sits at the top of its diameter tolerance.

Dies wear little by little in service, and that wear has been analysed together with the drawing conditions. In a study of dies from dry drawing of steel wire, wear was greatest where the wire enters and where the reduction zone meets the bearing (Haddi et al., 2012; Suliga et al., 2025). In the same study, the worn surface roughened, steel stuck to it or cracks formed, and the stress concentrated there could lead to die cracking and wire breaks. Wire that leaves a worn, oversize exit must be reduced that much more by the next die, so wear at one die shifts load onto the die after it. The die angle matters as much as wear. A small angle lengthens contact with the die and raises friction, a large one raises redundant work, so each reduction has a suitable angle. In simulations that raised the die angle from 6 to 14 degrees, contact pressure rose by about 50% on average, varying with location, and at reductions below 10% the large-angle dies wore over 30% more than the 6-degree die (Wright, 2016; Suliga et al., 2024). A large angle combined with a small reduction puts the centre of the wire in tension and can cause central bursts, rows of arrowhead-shaped cracks inside the wire. Analysis showed that under such a combination of angle, reduction and friction this defect can form in even the most ductile metal, and finite element models of aluminium alloy wire reproduced it (Avitzur, 1968; McAllen & Phelan, 2005).

Pull the dies before and after the break and examine them. Look for wear rings, cracks and stuck metal under a magnifier, and measure the wire diameter after each die against the designed pass schedule; that shows which die has grown and which die took on its share. Confirm die angle and bearing length from die records or with a profile gauge. If central bursts are suspected, cut an unbroken length along its axis, polish it and look for a row of arrowhead cracks at the centre.

For a die problem, revise the change rule first. Rather than going by hours or output alone, change a die when the wire diameter has grown by a set amount, and measure angle and bearing on reground dies before use. When dies from another line are mixed in, rework the pass schedule. If central bursts appear, redesign the angles and the reduction split with the die supplier so that no pass pairs a small reduction with a large angle.

Hypothesis 3: faulty pretreatment

Steel wire drawing starts only after the scale on the rod surface, the iron oxide skin formed in rolling, is removed and a coating that will hold the lubricant is applied. Scale is removed by pickling, dissolving it in acid, or mechanically, by bending the rod in several directions to crack the scale and brushing it off (Gillström & Jarl, 2006). Look at this hypothesis when the pickling acid is weak or loaded with iron, when rinsing or drying is rushed, or when control of the coating bath has slipped. A typical scene: in the week the acid is due for topping up, only the coils from one batch break one after another at the early dies. Their surface shows dark patches here and there, and a rub of the hand comes away with powder.

Pretreatment matters because the lubricant film ultimately stands on this surface. A zinc phosphate coating holds an even lubricant film over the whole surface, keeps metal from touching metal, and together with the lubricant stops steel from welding to the die or scoring during drawing. For that coating to form properly, the surface must first be clean, free of oil, rust and oxide. Smut, the black powdery residue left by pickling, can change the amount and crystal size of the coating, and a surface carrying pickling inhibitor residue coats poorly without strong alkaline cleaning (Narayanan, 2005). Where the coating is thin or patchy, the lubricant film breaks with it. Pickling can also weaken wire another way. In acid, a great many hydrogen atoms form on the metal surface and some enter the steel; the more hydrogen, the lower the ductility, and the loss grows with the strength of the steel (Louthan, 2008). Wire gains strength with every pass, so it moves towards the side more prone to this effect.

Examine the pickled rod surface first. If it is not an even matt grey but shows dark scale marks, or powder comes off on the hand, pickling or rinsing fell short. Check the acid strength, iron content, temperature and immersion time of the pickling bath against the records, and measure coating weight by stripping a set area and weighing the difference, then compare it with the supplier's recommended range. If breaks cluster in coils drawn straight after pickling, suspect hydrogen, and check whether a baking treatment to drive hydrogen out was done and under what conditions. Any hydrogen investigation should look at these bake-out records and the quality controls behind them (Louthan, 2008).

With the cause narrowed to pretreatment, rebuild the process control sheet. Measure acid and iron content in the pickling bath at fixed intervals and set rules for topping up and replacing it, and give only as much immersion time as it takes to lift the scale. Rinse well enough after pickling that no smut or acid stays behind, measure coating weight and keep it within range, and dry fully before drawing. For high-strength wire where hydrogen is suspected, agree with the rod supplier whether baking is needed and under what conditions, and adjust pickling so the rod is not left in acid too long.

Hypothesis 4: overheated lubricant

Hot weather, a speed increase to meet a delivery, and die cooling water lines that clog or lose flow are all times to check whether heat has built up. In wet drawing, where the wire passes through the dies immersed in lubricant, the same applies when the lubricant cooler falls short. Say a line ran without trouble all morning, then an hour or two after the speed went up a step, breaks began at the later dies. Soap at the die exit has turned darker than usual, smells burnt and sticks together in clumps.

Heat comes from deformation and friction. Most of the work spent reducing the wire and overcoming friction at the die face turns into heat, so a higher speed piles more heat into die and wire in the same time. In simulations of steel wire drawing, raising the speed from 1 to 5 metres per second made the deformation work per unit time about five times larger, and die and wire temperatures rose with it (Wright, 2016; Suliga et al., 2024). The same study explains that as the die heats up, the lubricant's flow properties deteriorate and the film thins, so the die wears faster, and in its friction tests the friction coefficient was higher at high temperature. In copper wire tests too, friction coefficient and the material's flow stress changed with speed, and temperature rise and drawing stress changed with them (Haddi et al., 2011). Since the thickness of a soap film depends on flow properties that change with heat, excess heat thins the film and can end by breaking down the lubricant on the wire, raising the drawing force and breaking the wire (Montmitonnet et al., 1982; Suliga et al., 2025).

Temperature shows itself as soon as it is measured. Measure the inlet and outlet temperatures and flow of the die holder cooling water and the surface temperature of the wire after each die with a contact or infrared thermometer, and check against the records whether breaks rise with speed and running time. Note the colour, smell and clumping of soap at the die exit as well. In wet drawing, compare lubricant temperature and concentration with the TDS ranges, and confirm from the temperature difference across the cooler that it is doing its job.

If heat is the cause, bring the cooling back first. Clean clogged cooling lines and filters and set the flow; if temperatures stay high after that, lower the speed or split the reduction of the die where heat builds up across the dies before and after it. If high speed is a must, review a change to a soap grade suited to high speed with the supplier; in tests, the speed that suited each soap differed by type (Felder et al., 2011). Scoop burnt soap out of the box, and in wet drawing bring the lubricant back within the TDS temperature and concentration ranges.

Hypothesis 5: flawed rod

Look at the rod when, with machine, lubricant and dies unchanged, breaks come only from certain coils or certain heat numbers. Watch for it closely right after a change of supplier or steelmaking lot, and in the last stages where wire is drawn very fine. Take two coils from the same supplier run on the same machine one after the other on the same day. One runs smoothly to the end, while the other breaks at one die and then another, and the breaks stop once the coil is changed.

Steel retains small amounts of non-metallic inclusions, such as oxides formed in steelmaking. A study of wire taken from each stage of a real drawing line tracked how inclusions change at every die and what microdefects form around them (Toribio et al., 2021). In wet drawing of fine high-carbon filaments, 90% of the broken filaments had an inclusion at the break, mostly silica or silica mixed with calcium or magnesium oxide, and fracture began as the inclusion came away from the surrounding steel (Godon et al., 2019). The same study reports that size and composition, not just the amount of inclusions, govern breaks, and that the size at which an inclusion causes a break depends on its composition. As wire gets finer, an inclusion of the same size takes up a larger share of the cross-section, so a flaw that was tolerated at earlier stages can become a problem in the last few dies.

The clue is in the broken end. Examine the fracture face under a magnifier for a small particle or hole where the break started, and if needed send it to a laboratory with scanning electron microscopy and chemical analysis. Group breaks by coil and heat number to see whether they cluster in one heat, and have the remaining rod rated with the standard test methods for inclusion content of steel (ASTM International, 2018). Check the rod surface for long, continuous flaws as well.

If the breaks cluster in one heat, set aside the remaining coils from that heat and ask the supplier for cleanliness data and the mill test certificate for it. Handing over the broken-end samples and coil records together makes it easier for the supplier to narrow the cause. For products where breaks keep recurring, agree with the supplier on adding an inclusion rating limit to the purchase specification.

Finding the cause

Five hypotheses do not mean five separate investigations. Rule them out one at a time, starting with what is easy to measure. The die box and cooling water can be checked without a long stop, and pickling and coating conditions are already in the records. Dies and rod need samples pulled for examination, so they come next.

The first clues are where and when the wire broke. Breaks that always come at the same die point to that die. Breaks that grow at the later dies with running time or after a speed increase point to an overheated lubricant and a thinning film; breaks at the early dies in coils pretreated in the same batch point to pretreatment; and breaks scattered across dies but only in certain coils or heats point to flawed rod.

Next is the shape of the break. If the wire stretched and necked before it broke, the pull exceeded the wire's strength, an overload, so look at what raises friction and heat: the lubricant film, the die and the lubricant temperature. Arrowhead cracks in a lengthwise section point to die angle and reduction, and a particle at the origin of the fracture to inclusions in the rod. Breaks that cluster in freshly pickled coils point to hydrogen taken up in pickling.

If that still does not settle it, run control trials that change one thing at a time. Put a coil from another heat on the same machine, fit a new die at the suspect position, refill the die box with freshly dried powder, and drop the speed one step. Change only one thing at a time, or there is no telling which one worked. Afterwards, count breaks per set output on the same basis as before the change, and the job is done only when that figure has recovered.

The hypotheses can overlap. A worn, roughened die face raises friction, friction turns into heat (Wright, 2016), and on a hot die the lubricant film thins and the die wears faster (Suliga et al., 2024). Wire with poor pretreatment holds less soap, so the lubricant film thins as well. In such cases, put lubrication and cooling right first and then look at die and rod again, because while lubrication and heat are unsettled, the effect of changing a die or a rod cannot be compared fairly.

Limits and cautions

Suitable drawing speed, reduction, die angle, coating weight, pickling conditions, and lubricant concentration and temperature differ by steel grade, wire size, machine and lubricant, so numeric decisions follow the lubricant's TDS and the machine and die suppliers' guidance. Inclusion analysis and judging hydrogen embrittlement are laboratory work, and for safety-related products such as spring wire or prestressing wire, do not release on floor judgement alone; get the rod supplier and the quality engineer to confirm.

Safety matters too. For pickling acids and coating chemicals, follow the product's safety data sheet, the SDS, for protective equipment and ventilation. Metalworking fluids such as wet drawing lubricants can harm health through skin contact and through breathing in mist (OSHA, n.d.). Handle soap powder so it does not become airborne, and clear or rethread broken wire only after the machine is fully stopped and locked out. Broken wire ends are sharp, so wear gloves and eye protection.

Sources

  1. ASTM International. (2018). ASTM E45-18a, Standard test methods for determining the inclusion content of steel. https://store.astm.org/e0045-18a.html
  2. Avitzur, B. (1968). Analysis of central bursting defects in extrusion and wire drawing. Journal of Engineering for Industry, 90(1), 79–90. https://doi.org/10.1115/1.3604608
  3. Felder, E., Levrau, C., Mantel, M., & Dinh, N. G. T. (2011). Experimental study of the lubrication by soaps in stainless steel wire drawing. Proceedings of the Institution of Mechanical Engineers, Part J: Journal of Engineering Tribology, 225(9), 915–923. https://doi.org/10.1177/1350650111415931
  4. Gillström, P., & Jarl, M. (2006). Mechanical descaling of wire rod using reverse bending and brushing. Journal of Materials Processing Technology, 172(3), 332–340. https://doi.org/10.1016/j.jmatprotec.2005.10.014
  5. Godon, J., Antoine, P., Vogt, J. B., & Bouquerel, J. (2019). Influence of steel cleanliness on drawability of fine filaments with high tensile strength. Metallurgical Research & Technology, 116(5), 513. https://doi.org/10.1051/metal/2019025
  6. Haddi, A., Imad, A., & Vega, G. (2011). Analysis of temperature and speed effects on the drawing stress for improving the wire drawing process. Materials & Design, 32(8–9), 4310–4315. https://doi.org/10.1016/j.matdes.2011.04.010
  7. Haddi, A., Imad, A., & Vega, G. (2012). On the analysis of die wear in wire-drawing process. Tribology Transactions, 55(4), 466–472. https://doi.org/10.1080/10402004.2012.671451
  8. Louthan, M. R. (2008). Hydrogen embrittlement of metals: A primer for the failure analyst. Journal of Failure Analysis and Prevention, 8(3), 289–307. https://doi.org/10.1007/s11668-008-9133-x
  9. McAllen, P., & Phelan, P. (2005). Ductile fracture by central bursts in drawn 2011 aluminium wire. International Journal of Fracture, 135(1–4), 19–33. https://doi.org/10.1007/s10704-005-3470-5
  10. Montmitonnet, P., Brison, M., & Delamare, F. (1982). Metallic soap lubrication in wire-drawing: A thermopseudoplastic model. Wear, 77(3), 315–328. https://doi.org/10.1016/0043-1648(82)90057-6
  11. Narayanan, T. S. N. S. (2005). Surface pretreatment by phosphate conversion coatings – A review. Reviews on Advanced Materials Science, 9, 130–177. https://eprints.nmlindia.org/337/
  12. Occupational Safety and Health Administration [OSHA]. (n.d.). Metalworking fluids. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/metalworking-fluids
  13. Suliga, M., Szota, P., Gwoździk, M., Kulasa, J., & Brudny, A. (2024). The influence of temperature in the wire drawing process on the wear of drawing dies. Materials, 17(20), 4949. https://doi.org/10.3390/ma17204949
  14. Suliga, M., Szota, P., Kulasa, J., Brudny, A., & Burdek, M. (2025). Friction and wear of tungsten carbide dies in the dry drawing of steel wire. Materials, 18(7), 1409. https://doi.org/10.3390/ma18071409
  15. Toribio, J., Ayaso, F.-J., & Rodríguez, R. (2021). Drawing-induced evolution of inclusions in cold-drawn pearlitic steel. Metals, 11(8), 1272. https://doi.org/10.3390/met11081272
  16. Wright, R. N. (2016). Wire technology: Process engineering and metallurgy (2nd ed.). Butterworth-Heinemann.

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.