KALTECKOREA

BlogApplication notes

Why do zinc-plated parts get white rust so soon?

Type
Application notes
Published
23 November 2026
Prepared by
Jonghwan Moon
Product group
Coatings & Surface Treatments

Asking for thicker plating is the usual response when white rust appears early, but delaying white rust is mainly the job of the conversion coating over the zinc and depends heavily on how long the parts stayed wet, so thicker plating alone tends to let it happen again. What actually lies behind it can be a thin or damaged conversion coating, overheated drying, damp storage, a missing sealer or thin zinc, and sometimes two or more at once.

Background

Zinc-plated brackets and bolts are boxed and left in the warehouse, and when the boxes are opened a few weeks later the surfaces are covered in white powder. The customer returns them as cosmetic rejects, and the word rust casts doubt on the whole lot. White rust is zinc oxide and zinc hydroxide formed as zinc corrodes, and it takes up roughly three to five times the volume of the zinc metal, so it looks worse than it is. White rust formed in storage is unsightly but often costs little zinc, though the longer the parts stay wet, the more zinc is lost (AGA, 2014).

Zinc plating protects steel sacrificially: zinc corrodes before the steel and so shields it (Zhang, 1996). That makes zinc a reactive metal, so after plating it is dipped in a chromium compound solution to form a conversion coating, a thin protective film made by converting the zinc surface itself, which delays white rust. The zinc plating specification sets, for each type of supplementary treatment, how long the parts must go in a salt spray test without zinc corrosion products, and has the plating thickness chosen by the class of service environment (ASTM International, 2023).

Early white rust means the coating did not do its job, the parts stayed wet too long, or there was too little zinc to protect. In the atmospheric corrosion of zinc, the pH of the surface water film governs how fast the protective layer on the zinc dissolves, and indoors corrosion can be held very low by keeping relative humidity moderate (Graedel, 1989).

In such cases the technical team sets up the five hypotheses below and rules them out one by one. The start is always the same: compare the plating callout on the drawing, meaning thickness class, type of supplementary treatment and whether a sealer is required, with the plating certificate and the actual process records, and log the drying, packing, storage and transport conditions after plating, with dates.

Hypothesis 1: thin or damaged coating

Look at this hypothesis first when the concentration, pH or temperature of the conversion bath has drifted out of range, when a long-used bath has built up dissolved zinc and iron, when immersion time has been cut, or right after a switch from hexavalent to trivalent chromium treatment. Processes that pour small barrel-plated parts into a large bin before the coating dries belong here too. Picture wet screws, just out of the conversion bath, tipped by the basket into a transport bin. When the lot is opened a few weeks later, white spots have come up first on the head edges and thread tips that knocked against each other.

Conversion coatings are very thin. In one study, a 1-minute immersion produced a coating about 400 nm thick from a hexavalent chromium bath and about 90 nm thick from a commercial trivalent chromium bath. In the same study the trivalent coating still inhibited zinc corrosion considerably, but less than the hexavalent one, and the difference was explained by coating thickness and by whether mobile hexavalent chromium species were present to repassivate flaws (Zhang et al., 2005). In a thin film with nothing to heal its own flaws, any spot where a slightly off process left the film underdeveloped, or where the soft wet film was scratched or pressed, stays bare zinc. When moisture reaches it, white rust comes up there first.

Open the conversion bath analysis records first. Check concentration, pH, temperature and immersion time against the TDS ranges, and note when the bath was last made up and how much work it has processed since. For coloured coatings, see whether the colour is even across the lot, and use a magnifier to see whether the white spots follow impact marks or scratches. Measure coating performance with a salt spray test and compare it with the hours set for that treatment type (ASTM International, 2023, 2026).

If the bath is the cause, reset the analysis interval and the rules for topping up and renewal, and keep immersion time to what the TDS specifies. For barrel parts, bring drying forward or change the handling so parts do not knock together or get poured until the coating has dried. After a switch from hexavalent to trivalent, decide again with the supplier whether the trivalent treatment type meets the required salt spray hours and whether a sealer should be added.

Hypothesis 2: overheated drying

This hypothesis comes up when drying temperature after conversion coating has been raised, when the hot air in a centrifugal dryer has grown hotter, or when coated parts go through a later process that heats them again, such as baking against hydrogen embrittlement after conversion coating, or an oven that cures paint or adhesive. Suppose there was a week when the dryer setting was turned up a few steps to meet a delivery. The parts looked fine straight after drying, but a few weeks after shipment, white rust complaints come in for the lots made that week only.

A conversion coating holds water, and that water supports the film's properties. In a study that dried hexavalent- and trivalent-treated electrogalvanised steel at three temperatures between 60 °C and 210 °C, both coatings dehydrated during heating, and heating above 110 °C could severely reduce the corrosion protection both treatments gave. The hexavalent coating also degraded through widening cracks and reduction of hexavalent chromium to the trivalent state (Zhang et al., 2006). Even when the surface looks almost unchanged, water leaves the film and gaps open inside it, so the coating holds out for a shorter time once moisture arrives.

Measure the temperature of the parts themselves, not the dryer display. Put parts fitted with a thermocouple or a temperature indicator label into the dryer to find how hot they actually get, and compare that with the maximum drying temperature in the conversion coating's TDS. Look through the process flow for any heat step after conversion coating, such as baking, paint curing or shrink fitting. Putting samples from the same lot dried at a lower temperature into the salt spray test alongside makes the difference visible in numbers.

If overheating is confirmed, bring drying temperature back below the TDS limit and add a regular check of part temperature to the work instructions. For parts that need baking against hydrogen embrittlement, change the sequence so baking comes straight after plating and before conversion coating. The specification also requires that, where baking is needed, it is done before supplementary treatments (ASTM International, 2023). For parts that cannot avoid heat after conversion coating, choose a heat-resistant treatment with the supplier.

Hypothesis 3: damp storage

Consider this hypothesis when parts were sealed in plastic before they were fully dry, when still-warm parts went straight into boxes, when shipments passed through humid periods such as the rainy season or a sea voyage, or when parts moved from a cold warehouse into a warm shop and dew formed on them. Parts that stack against each other, such as washers and flat plates, are more exposed. Picture a rainy-season afternoon: parts fresh from the dryer are bagged, boxed and moved to a cool warehouse. A few days later droplets have formed inside the bags, and white powder sits on the faces where parts touch and on the parts at the bottom of the bag.

Where air moves freely, a zinc surface goes through wetting and drying, and zinc hydroxide meets carbon dioxide in the air to form a thin, compact layer of zinc carbonate. When water is trapped between parts with no airflow, however, the oxygen supply differs between the middle and the edge of a droplet, a corrosion cell forms, and with oxygen the carbon dioxide supply is also cut off, so zinc hydroxide that cannot turn into carbonate keeps piling up as white powder (AGA, 2014). In one experiment with salt-dosed zinc at 95% relative humidity, zinc oxide was the main corrosion product without carbon dioxide, while basic zinc carbonates and a chloride-bearing zinc compound dominated with it (Lindström et al., 2000). So even with the same coating, white rust comes up quickly when parts sit long in trapped water.

Where the white rust sits is the first clue. If it gathers on faces where parts touch, at the bottom of bags or boxes and on the inner faces of stacked parts while outer surfaces exposed to air are clean, give this hypothesis weight. Check the part temperature and dryness at packing, whether the packaging breathes or is sealed, and the warehouse temperature and humidity records. If there are no records, put temperature and humidity loggers in the warehouse and in shipping boxes so numbers are kept from the next shipment on.

Once the cause narrows to moisture, change packing and storage. Dry parts fully and let them cool to room temperature before packing, and put a desiccant in sealed packs. In the warehouse, keep parts off the floor, avoid close stacking and leave gaps so air can pass, and when parts move to a place with a large temperature difference, leave them packed until they reach temperature rather than opening them at once. If condensation in transit is a concern, use covers and spacers so water cannot collect.

Hypothesis 4: missing sealer

A sealer is a thin film applied over the conversion coating. Suspect this hypothesis when a switch from hexavalent to trivalent chromium left the treatment callout on the drawing unchanged, when the sealer bath has weakened or immersion was short, or when strong solvent in pre-assembly cleaning has stripped the sealer. A part that gave no trouble for years in the same warehouse and packaging, but draws white rust complaints from the lots made after the process change, is a case in point. Set old and new lots side by side and only a slight difference in colour and gloss tells them apart.

A sealer's job is to cover the weaknesses of a thin conversion coating. In a study comparing industrially produced zinc from a cyanide-free alkaline bath with trivalent chromium treatment against hexavalent treatment, the hexavalent coatings performed better overall, but the trivalent coating with a sealing treatment behaved comparably to hexavalent treatment without sealant. That sealing treatment formed a layer made mainly of a mixed organic and inorganic matrix (Bellezze et al., 2024). As seen earlier, a trivalent coating is thin and lacks species that heal its own flaws, so without a sealer nothing makes up for that. A trivalent coating left on its own and expected to resist white rust as the old hexavalent one did will show white rust earlier, by the size of that gap.

Start by reconciling the paperwork. Check whether the drawing and purchase specification call for a sealer or topcoat, whether the plating certificate records a sealing step, and whether the timing of the process change matches the lots with white rust. If the process uses a sealer, compare sealer bath concentration, temperature, immersion time and drying conditions with the TDS. If parts are washed before assembly, ask the supplier whether that cleaner dissolves the sealer. Finally, put sealed and unsealed samples into the same salt spray test and compare the time to white rust.

If a sealer is judged necessary, choose a sealer or topcoat suited to the service environment and the required salt spray hours with the supplier, and write the requirement into the drawing and purchase specification as performance rather than a product name. Give the sealer bath an analysis interval and topping-up rules, as for the conversion bath. For threaded parts such as bolts, check at the same time whether an added sealer or topcoat changes the tightening conditions. Switch pre-assembly cleaning to a cleaner that does not harm the sealer.

Hypothesis 5: thin zinc

Thin zinc becomes the problem when the thickness class chosen is lower than the service environment calls for, when thickness varies from part to part as in barrel plating, when a part has many places current struggles to reach such as thread roots and recesses, or when parts serve where chlorides are plentiful, such as the coast or winter roads. Take a part supplied both to an inland plant and to a coastal site. White rust spreads quickly only on the parts sent to the coast, and red rust soon shows in thread roots and recesses.

Zinc protects steel by being consumed, so the protection lasts as long as zinc remains, and the time a zinc coating lasts before first maintenance is proportional to its thickness (AGA, 2014). The zinc plating specification therefore splits thickness classes by service environment, with thicker classes for harsher ones, such as 5 µm for mild and 8 µm for moderate conditions (ASTM International, 2023). Thickness also varies within one part. In electroplating, current concentrates on edges and projections and reaches recesses less, so thickness differs from place to place on the same part (Dukovic, 1990). Even when the average thickness meets the class, thread roots and recesses can be thin, and the zinc there turns to white rust and is used up first.

Thickness simply needs measuring. Measure it by X-ray fluorescence separately on flat faces, edges, thread roots and inside recesses (ASTM International, 2021), and see whether the thinnest spot meets the class on the drawing. Measure several parts from the lot to see the spread between parts as well. Re-examine the service environment against the international classification of atmospheric corrosivity, which grades environments by how much standard metals corrode in the first year (ISO, 2012), and confirm that the chosen thickness class suits it.

If thickness is short, first raise the class to suit the environment, and state on the drawing where it is measured rather than an average. For parts whose thread roots or recesses are always thin, review a move to rack plating, or changes to auxiliary anodes and racking, with the plating supplier. If even a thicker coating cannot cope with the environment, consider a different coating system, such as a zinc alloy, with the supplier.

Finding the cause

The five hypotheses need not be tested all at once. Rule them out one at a time, starting with what is easy to measure. Packing and storage conditions, drying temperature records, and the treatment and sealer callouts on the drawing and certificate can be checked today, and thickness can be measured within hours. Salt spray tests take days, so run them after the earlier checks have narrowed the field.

The first clue is where and when the white rust appeared. If it gathered on faces where parts touch or at the bottom of packs, and appeared after transport or the rainy season, look at damp storage; if it came up evenly over every surface of a whole lot, look at the coating or the drying temperature. If it appeared only in lots that saw more heat or in parts that went through a heat step, lean towards overheating, and if it follows impact marks, suspect damage to the wet coating. If it starts in thread roots and recesses and soon leads to red rust, look at thin zinc, and if it began with the lots after a process change, look at the sealer or the trivalent coating.

If that still does not settle it, split one lot for control trials. Keep one half on current conditions and change only one thing in the other, such as lower drying temperature, an added sealer or breathable packaging. Comparing the time to white rust side by side, in a salt spray test or in the same warehouse, shows which condition made the difference. Afterwards, count white rust complaints per shipped lot on the same basis as before the change.

The hypotheses can overlap. A part with a thin trivalent coating and no sealer shows white rust when only a little moisture is trapped in storage, and a coating dried out by overheating gives way faster in the same moisture. In thin thread roots, once the coating's time is up, the remaining zinc goes quickly too. In such cases, put storage and packing right first and then look again at the coating, drying temperature, sealer and thickness, because while moisture is unsettled, the effect of changing the coating or sealer cannot be compared fairly.

Limits and cautions

Control ranges for the conversion bath, maximum drying temperature, sealer conditions and thickness classes differ by chemistry and specification, so numeric decisions follow the product's TDS and the drawing specification. Use salt spray tests to compare coatings under identical conditions, not to predict service life on their own. The test practice itself notes that salt spray results used alone have seldom correlated with performance in natural environments (ASTM International, 2026). Whether white rust affects function, and whether the parts can be used as they are, is for the customer specification and the quality engineer to decide.

Safety matters too. Hexavalent chromium compounds are classed as carcinogens with their own exposure controls, so when handling hexavalent conversion solutions, follow those rules and the SDS for protective equipment and ventilation (OSHA, n.d.). For trivalent solutions, sealers and the acids used to strip plating, wear gloves and eye protection as each product's SDS directs. Keep white rust powder from becoming airborne when brushing it off, and run the salt spray cabinet to its set procedure.

Sources

  1. American Galvanizers Association [AGA]. (2014). A guide to minimizing and treating wet storage stain on hot-dip galvanized steel. https://galvanizeit.org/uploads/publications/Wet_Storage_Stain_On_Galvanized_Steel.pdf
  2. ASTM International. (2021). ASTM B568-98(2021), Standard test method for measurement of coating thickness by X-ray spectrometry. https://store.astm.org/b0568-98r21.html
  3. ASTM International. (2023). ASTM B633-23, Standard specification for electrodeposited coatings of zinc on iron and steel. https://store.astm.org/b0633-23.html
  4. ASTM International. (2026). ASTM B117-26a, Standard practice for operating salt spray (fog) apparatus. https://store.astm.org/b0117-26a.html
  5. Bellezze, T., Fratesi, R., & Roventi, G. (2024). Morphological characterisation and corrosion resistance of Cr III- and Cr VI-based conversion layers on zinc coatings. In Electrochemical approach to selected corrosion and corrosion control studies (EFC 28) (pp. 180–192). CRC Press. https://doi.org/10.1201/9781003580058-16
  6. Dukovic, J. O. (1990). Computation of current distribution in electrodeposition, a review. IBM Journal of Research and Development, 34(5), 693–705. https://doi.org/10.1147/rd.345.0693
  7. Graedel, T. E. (1989). Corrosion mechanisms for zinc exposed to the atmosphere. Journal of The Electrochemical Society, 136(4), 193C–203C. https://doi.org/10.1149/1.2096868
  8. International Organization for Standardization [ISO]. (2012). ISO 9223:2012, Corrosion of metals and alloys — Corrosivity of atmospheres — Classification, determination and estimation. https://www.iso.org/standard/53499.html
  9. Lindström, R., Svensson, J.-E., & Johansson, L.-G. (2000). The atmospheric corrosion of zinc in the presence of NaCl: The influence of carbon dioxide and temperature. Journal of The Electrochemical Society, 147(5), 1751. https://doi.org/10.1149/1.1393429
  10. Occupational Safety and Health Administration [OSHA]. (n.d.). Hexavalent chromium. U.S. Department of Labor. Retrieved November 2026. https://www.osha.gov/hexavalent-chromium
  11. Zhang, X. G. (1996). Galvanic corrosion of zinc and its alloys. Journal of The Electrochemical Society, 143(4), 1472–1484. https://doi.org/10.1149/1.1836662
  12. Zhang, X., van den Bos, C., Sloof, W. G., Hovestad, A., Terryn, H., & de Wit, J. H. W. (2005). Comparison of the morphology and corrosion performance of Cr(VI)- and Cr(III)-based conversion coatings on zinc. Surface and Coatings Technology, 199(1), 92–104. https://doi.org/10.1016/j.surfcoat.2004.12.002
  13. Zhang, X., van den Bos, C., Sloof, W. G., Hovestad, A., Terryn, H., & de Wit, J. H. W. (2006). Drying effects on corrosion properties of Cr(VI)- and Cr(III)-treated electrogalvanized steel. ECS Transactions, 1(9), 165–176. https://doi.org/10.1149/1.2215586

Product and site consultation

Leave your company, site and the product groups in use. Our engineer will get in touch to go through your site conditions and concerns. Materials, equipment, operating conditions and downstream steps show what should change and what can stay. If nothing needs to change, we will say so.

Contact us
After you contact us
  1. 01
    Site setup

    We confirm process conditions and needs first.

  2. 02
    Spec design

    We set the product spec and selection criteria.

  3. 03
    Comparison

    We compare matching candidates and propose.

  4. 04
    Tailored supply

    We supply on time and manage the stock.

  5. 05
    Site check

    We visit, check conditions of use and record.

  6. 06
    Use management

    We track use and change cycles to catch issues.

  7. 07
    Regular analysis

    We analyze the records and send a yearly report.