Customer storiesPrecision drive-component maker for automation and industrial machinery
A drive-parts maker eased pre-paint cleaning with residue-free storage protection

- Customer
- Precision drive-component maker for automation and industrial machinery
- Industry
- Machinery & Precision Machining, Robotics & Logistics Automation
- Product group
- Corrosion Prevention
- Process · Material
- Work-in-process storage protection and pre-paint preparation · Steel for precision drive components (carbon and alloy steel)
A maker of precision drive components that runs design through after-sales service in-house changed how it judges rust protection for parts stored between operations: by what it does to washing and painting as well. Having traced post-wash stains and rust to residual rust-preventive oil and incomplete sealing, it moved to a low-residue rust preventive with zipper-seal VCI film, holding back summer rust and simplifying pre-paint cleaning.
The customer is a specialist manufacturer of precision drive components that runs design, manufacturing, testing and after-sales service as one flow. It makes precision parts in many sizes for automation equipment and industrial machinery, and each part moves between operations and through interim storage on its way to becoming a finished product. Integrated production is a strength, and it also means the company owns the waiting time between operations, which is why cleanliness and surface condition in storage are core control items.
The last operation is painting. Parts leave storage, go through washing and then on to paint, so the rust protection chosen for storage carries through to washing and paint quality. The customer therefore set a standard of judging storage protection by what it does to the operations that follow, not by storage alone.
Parts had to stay free of rust through storage even in a hot, humid summer warehouse, come out of the post-storage wash without stains or rust, and need less, or simpler, degreasing before painting. Sealing also had to be reliable and done the same way whatever the part size or quantity. Under that standard, storage, washing and painting become one surface-management flow.
The challenge: stains and summer rust that survived every change to the wash
Until then parts were coated with a non-water-soluble rust-preventive oil and stored in one of three ways depending on the situation. They went into a VCI plastic bag inside a box, into a VCI bag inside a case box, or into an open box. Each method had its advantages, but the same things kept happening with all three. When summer humidity rose, oiled parts still rusted, stains and rust showed on the surface after washing, and degreasing before painting could never be skipped.
“We changed the wash who knows how many times and the stains still came out, so we kept staring at the wash. It was only when we heard the oil from storage was the problem that we went back and looked at the earlier step.”Paint process lead, customer
In week zero the customer asked for a look at three things together: summer rust in storage, stains after washing and the pre-paint cleaning burden. The three showed up in different operations, but they were happening on the same surface of the same parts. So before touching the wash conditions again, the customer and our team decided to follow that surface from the moment a part went into storage to the moment it reached the wash.
The solution: changing the oil and the seal in storage, not the wash
In weeks one and two the customer and our team compared where rust appeared under each of the three storage methods and checked warehouse humidity, the state of the bag seals and where stains appeared after washing. Summer rust showed first in bundles with poorly sealed bags and in open-box storage, and some bags had droplets on the inside. Post-wash stains clustered on lower faces and around holes where the oil had pooled thickest. The places where rust and stains appeared matched the storage method far better than the wash conditions.
An oil film protects only what it covers. A rust-preventive oil works by laying a film on the metal that keeps out moisture and oxygen, so protection breaks at edges where the film is thin, where hands touched the part and over moisture that was there before oiling. In a summer warehouse, warm humid daytime air trapped in a bag cools at night past its dew point, and condensation forms on the inside of the bag and on the parts. If the seal is incomplete, humid air keeps moving in and out and the cycle repeats, so rust becomes more pronounced the longer parts are stored.
Leftover oil unsettles washing and painting. Rust-preventive oil stored for a long time partly oxidizes, turns tacky and does not wash off evenly. Where oil remains in islands, rinse water beads and dries into stains, and where the oil came off first, bare wet metal waits to dry and flash rust appears. Painted in that state, the residual oil lowers surface energy, the paint cannot wet evenly and adhesion suffers. However the wash conditions were changed, this would recur as long as the oil stayed, so the post-wash stains and rust started not with the wash but with the oil the rust preventive left behind.
In week three the causes were pinned down as two. One was incomplete sealing and trapped moisture, and the other was residual rust-preventive oil that washing does not remove evenly. The comparison therefore moved from the cleaner to the storage protection itself, and was made by working principle rather than by brand. The options were an oil film that covers the surface, a low-residue dry film with vapor-phase protection added, and sealing solved by the structure of the pack rather than by each operator's technique. The shortlist narrowed to a low-residue rust preventive combined with zipper-seal VCI film.
The rust preventive's carrier solvent flashes off quickly after application, leaving little residue, and its vapor-phase inhibitors and film formers work together to leave a clear, dry film with no oily residue. It contains no chlorine compounds, chromate or nitrite, has a low VOC of 4.0 g/l, uses a non-flammable solvent, is applied by spray or dip and protects for up to 2 years in indoor storage. The film is a dedicated zipper-seal film with built-in vapor-phase inhibitor, which vaporizes inside the closed pack, fills the space and adsorbs on metal as a molecular layer that reaches gaps and holes an oil film never touches. The zipper makes sealing easy and reliable, keeping out outside moisture and contamination, and the film releases inhibitor continuously so the concentration inside the pack holds even in humid summers. With VCI packaging reliable sealing is part of the performance, so this structure takes on the first cause directly.
Adoption: from a summer-long in-house storage trial to one storage standard
Parts are packed clean and dry and handled with gloves so no fingerprints are left. Before full adoption the customer verified the combination with its own trial. From week four to week eleven, for about two months including the summer, it compared corrosion protection and residual contamination against the old methods under the same conditions as real storage. After confirming satisfactory results, the customer decided to adopt the combination formally for work-in-process storage.
Formal adoption began in the third month, and the WIP storage standard was unified on the new combination. Oiling a part and then choosing between a bag, a case box and an open box became a single sequence of low-residue rust preventive followed by zipper-seal VCI film. Whatever the part size or quantity, sealing is the same motion of closing a zipper, which leaves less room for seal quality to vary from one operator to the next.
The results: three storage methods down to one, and lighter pre-paint cleaning ahead
The wash was the first place the difference showed. With little residual oil, the cause of post-wash stains and rust was removed, and the process moved toward needing less separate degreasing before painting. In the warehouse the zipper film structurally solves incomplete sealing, so the summer rust that used to appear even on oiled parts is held back and conditions inside the pack stay constant in humid weather. Three storage methods became one combination, handled the same way by every operator.
For a supplier to makers of automation equipment and industrial machinery, paint quality is both appearance and corrosion resistance. Managing surface condition as one flow from storage to paint means paint problems are now stopped near the front of the process. The coating the customer's own customers receive now depends less on warehouse humidity or on how carefully each bag was sealed.
“Every summer we'd see droplets inside the bags, wipe the parts down and oil them again. Now you just close the zipper properly. The paint side talks about wash time a lot less too.”Materials and storage lead, customer
What's next: finding out how far pre-paint cleaning can be cut
The direction toward simpler pre-paint cleaning is confirmed, but how far it can go depends on part geometry and paint specification. The customer and our team are looking at checking paint adhesion on coupons with reduced wash steps for each part family, in order to reset the cleaning standard. They are also weighing whether to extend the same combination to shipping packaging and export transport.